Ferrite Toroid Core: Copper-Zinc Ferrite Sintered at 1100 °C, Presintered Twice at 900 °C (Snoek 1948, Ex. I)
A soft ferrite ring core for coils and transformers: copper, zinc and iron oxides with a little brownstone, presintered twice at 900 °C, pressed into a ring and sintered at 1100 °C in oxygen. Snoek's ring had an initial permeability of 154.
Source: J. L. Snoek, US 2,452,530 (Philips, 1948), Example I and its table. The violet iron oxide has its own blueprint (precipitated hematite calcined at 1000-1100 °C, after Nurdini et al. 2022); Snoek does not say how his was made. Picture: the patent's Fig. 4, the ring core.
Продвинутый
2 days
Инструкции
1
1
Weigh 20 : 30 : 50 mol % and 1 % brownstone
Weigh 20 : 30 : 50 mol % and 1 % brownstone
Mix 20 mol % pure copper oxide, 30 mol % pure zinc oxide and 50 mol % pure violet iron oxide, and add 1 % by weight of brownstone (manganese dioxide). Ours, by weight: 13.24 g copper oxide, 20.32 g zinc oxide and 66.44 g iron oxide per 100 g, plus 1 g brownstone. Snoek does not say what makes it 'violet'; violet iron oxide has its own blueprint.
Материалы для этого шага:
Оксид меди13.24 г
Порошок оксида цинка20.32 г
Фиолетовый оксид железа66.44 г
Диоксид марганца (пиролюзит)1 гНеобходимые инструменты:
Рычажные весы
Противопылевая маска2
2
Grind half an hour in an iron ball mill
Grind half an hour in an iron ball mill
Grind the mixture for half an hour in a mill with iron balls.
Необходимые инструменты:
Железная шаровая мельница
Противопылевая маска3
3
Presinter at 900 °C for 2 hours in oxygen
Presinter at 900 °C for 2 hours in oxygen
Heat the ground powder to 900 °C for 2 hours in oxygen and let it cool.
Необходимые инструменты:
Трубчатая печь
Кислород
Баллон для газа под давлением
Пирометр
Тигель с крышкой (фарфоровый)
Термостойкие перчатки4
4
Grind and presinter at 900 °C again (2 of 2)
Grind and presinter at 900 °C again (2 of 2)
Grind the powder, then heat it once more to 900 °C in oxygen. Snoek gives no times for the repeats.
Необходимые инструменты:
Железная шаровая мельница
Трубчатая печь
Кислород
Баллон для газа под давлением
Тигель с крышкой (фарфоровый)
Термостойкие перчатки
Противопылевая маска5
5
Grind 2 hours with iron balls
Grind 2 hours with iron balls
Grind it for 2 hours in a disintegrator with iron balls.
Необходимые инструменты:
Железная шаровая мельница
Противопылевая маска6
6
Press a ring at 4 tons per cm²
Press a ring at 4 tons per cm²
Press the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm cross-section.
Необходимые инструменты:
Гидравлический пресс
Пресс-форма для колец
Противопылевая маска7
7
Sinter at 1100 °C in oxygen, cool 5–10 °C a minute
Sinter at 1100 °C in oxygen, cool 5–10 °C a minute
Sinter the ring at 1100 °C in a current of oxygen. Example I heats for 1 hour and cools in the oxygen at 5 to 10 °C per minute. Snoek's ring had an initial permeability of 154, measured at room temperature at 2 kHz.
Необходимые инструменты:
Трубчатая печь
Кислород
Баллон для газа под давлением
Пирометр
Щипцы для тигля
Термостойкие перчаткиМатериалы
4- 13.24 гЗаполнитель
- 20.32 гЗаполнитель
- 66.44 гЗаполнитель
- Заполнитель
Требуемые инструменты
12- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
По этому чертежу делают
Связанные чертежи
Эти чертежи делятся знаниями — техники, материалы или принципы
CC0 Общественное достояние
Этот чертёж выпущен под лицензией CC0. Вы можете свободно копировать, изменять, распространять и использовать эту работу в любых целях без запроса разрешения.
Поддержите мейкера, покупая товары через его чертёж, где он получает Комиссию мейкера установленную продавцами, или создайте новую итерацию этого чертежа и включите его как связь в свой чертёж для распределения дохода.