Fused Quartz Tube: Blown from Brazil Pebble in the Oxy-Gas Flame (Shenstone, 1916)
Charlie

Создано

Charlie

4. ноябрь 2026DE
11
0
0
0
0

Fused Quartz Tube: Blown from Brazil Pebble in the Oxy-Gas Flame (Shenstone, 1916)

Fused silica stands sudden heating and cooling that would crack glass, but natural quartz splinters violently in a flame. W. A. Shenstone, in The Methods of Glass-Blowing and of Working Silica in the Oxy-Gas Flame (1916), first turns Brazil pebble into a "non-splintering" silica by quenching it from a yellow-red heat, then melts it in an oxy-gas flame into fine rods, wraps the rods round a platinum core into a first tube, and enlarges it with rings of rod blown out. Not given: quantities and times. He advises most workers to start from bought tubes and to learn each stage by practice. Source: W. A. Shenstone (1916), pp. 88-94. Picture: his p. 93.
Продвинутый
Several days of practice

Инструкции

1

Read Shenstone

"The silica tubes thus made can be cut and broken like glass, they can be joined together before the flame, and they can also be drawn into smaller tubes when softened by heat."
2

Crack the Brazil pebble

Clean the chips of Brazil pebble (rock crystal) thoroughly, heat them in boiling water and drop them into cold water. Repeat until they have cracked enough to break easily with a clean steel pestle or hammer. Hand-pick the fragments and reject any that are not perfectly free from foreign matter.

Материалы для этого шага:

Горный хрустальГорный хрусталь1 as required
ВодаВода1 as required

Необходимые инструменты:

Кастрюля с высокими стенкамиКастрюля с высокими стенками
ЭлектроплиткаЭлектроплитка
ВедроВедро
Слесарный молоток с шаровым бойкомСлесарный молоток с шаровым бойком
3

Make it non-splintering

Heat the pure, transparent pieces to a yellow-red heat in a covered platinum dish in a muffle furnace and plunge them quickly into a deep clean vessel of distilled water. Repeat until they are semi-opaque, friable masses like white enamel. Wash them with distilled water, drain and dry. Now they can go straight into the hottest part of the flame without splintering.

Материалы для этого шага:

Дистиллированная водаДистиллированная вода1 as required

Необходимые инструменты:

Платиновая чашкаПлатиновая чашка
Муфельная печьМуфельная печь
Щипцы для тигляЩипцы для тигля
Стеклянный стакан (химический)Стеклянный стакан (химический)
4

Set up the flame

Use an efficient oxy-gas burner fed with coal gas and oxygen from a bottle fitted with a gauge and regulator; watch the oxygen used. Protect your eyes with very dark glasses, so dark that work is a little difficult at first, and keep a second pair for long spells, as the glasses get hot. The hottest spot is near the tip of the inner cone: bring the work exactly there.

Материалы для этого шага:

Светильный газСветильный газ1 as required
КислородКислород1 as required

Необходимые инструменты:

Кислородно-газовая горелкаКислородно-газовая горелка
Баллон для газа под давлениемБаллон для газа под давлением
Редуктор давленияРедуктор давления
МанометрМанометр
Затемнённые очки для горнаЗатемнённые очки для горна
5

Draw fine rods

Hold a fragment in platinum-tipped forceps and melt one corner. Press a second fragment against the melted part until they stick, and heat from below upwards (to avoid bubbles) until it is clear. Add a third, a fourth and so on until you have an irregular rod. Reheat it in sections and draw it out into rods or coarse threads 1 to 2 mm across.

Необходимые инструменты:

Пинцет с платиновыми наконечникамиПинцет с платиновыми наконечниками
Кислородно-газовая горелкаКислородно-газовая горелка
Затемнённые очки для горнаЗатемнённые очки для горна
6

Make the first tube

Bind a few rods round a platinum rod about 1 mm across with platinum wires at both ends. Withdraw the core slightly from one end and heat gradually from there until a rough tube 4 to 5 cm long has formed. Close one end, blow it into a small bulb, fix a silica rod to the far end of the bulb, reheat and draw it out into a fine tube. Blow a fresh bulb on one end and draw it out again, until the tube is 6 to 8 cm long.

Необходимые инструменты:

Платиновая проволокаПлатиновая проволока
Пинцет с платиновыми наконечникамиПинцет с платиновыми наконечниками
Кислородно-газовая горелкаКислородно-газовая горелка
Затемнённые очки для горнаЗатемнённые очки для горна
7

Blow without soiling it

Blow through a rubber tube on the open end of the silica tube, with a glass tube loosely packed with granulated potash between your mouth and the work so the inside stays clean. Do not take a hot bulb out of the flame to blow it; move it just off the hot spot. Mend holes with plastic silica from the softened end of a fine rod and blow the lump out. Keep the silica clean: a white crust that forms is removed by reheating, but dust or handling can spoil the surface for good.

Необходимые инструменты:

Резиновая трубкаРезиновая трубка
Стеклянная трубкаСтеклянная трубка
Карбонат калия (поташ)Карбонат калия (поташ)
Кислородно-газовая горелкаКислородно-газовая горелка
8

Enlarge and lengthen

To widen a bulb into a tube, lay a ring of fine rod round its end, heat the ring and the end until soft and blow; repeat until the bulb becomes a short tube. For a long tube make several pieces 200 to 250 mm long at the diameter you need and join them end to end. Thicken a tube by adding rings and blowing them out. For a large tube, set a plate of silica behind the work to throw the flame back onto its far side.

Необходимые инструменты:

Кислородно-газовая горелкаКислородно-газовая горелка
Пинцет с платиновыми наконечникамиПинцет с платиновыми наконечниками
Затемнённые очки для горнаЗатемнённые очки для горна
9

History and honest limits

Thorpe's Dictionary (vol. IV, 1913) records Gaudin spinning fused silica threads in 1839, Boys making quartz fibres in 1887, and Shenstone showing in 1901 how to make tubes and bulbs before the oxy-coal-gas blowpipe. Shenstone gives no quantities or times and says most workers save time and money by starting from bought silica tubes. A finished tube holds a little moisture and nitric peroxide; he removes them by heating it and drawing filtered air through, not by washing.

Материалы

5

Требуемые инструменты

18

CC0 Общественное достояние

Этот чертёж выпущен под лицензией CC0. Вы можете свободно копировать, изменять, распространять и использовать эту работу в любых целях без запроса разрешения.

Поддержите мейкера, покупая товары через его чертёж, где он получает Комиссию мейкера установленную продавцами, или создайте новую итерацию этого чертежа и включите его как связь в свой чертёж для распределения дохода.

Обсуждение

(0)

Войти чтобы присоединиться к обсуждению

Загрузка комментариев...