Rasps: Teeth Raised One at a Time with a Pointed Punch
A rasp is a coarse file whose teeth stand separately instead of in continuous rows. Each tooth is raised by driving a pointed punch into the face of the blank at uniform distances. Because the teeth stand apart, a rasp clogs less than a cut file on soft material such as wood or a horse's hoof. The blank is forged, annealed and ground like a file blank, and the finished rasp is hardened like a file: coated against scale, brought to a dull red heat and plunged into water, with the tang tempered so it will not snap. Machine-made rasps have uniformly stamped teeth, which line up row behind row and leave deeper marks; slightly uneven hand-cut teeth avoid this.
Продвинутый
2 days (annealing overnight)
Инструкции
1
1
Forge the blank
Forge the blank
Forge the steel to a tapered bar, flat, round or half-round, with a narrow pointed tang at one end.
Материалы для этого шага:
Заготовка из высокоуглеродистой стали0.5 кгНеобходимые инструменты:
Кузнечный горн
Наковальня
Кузнечный молот
Кузнечные клещи2
2
Anneal and grind
Anneal and grind
Anneal the blank soft so the teeth can be raised, then grind the faces to a smooth, clear surface.
Необходимые инструменты:
Кузнечный горн
Точильный круг3
3
Punch the teeth
Punch the teeth
Drive the pointed punch into the face with the hammer at uniform distances, raising one separate tooth at each blow. Turn the rasp over on a soft metal plate to work the other face without crushing the finished teeth.
Необходимые инструменты:
Насечное зубило для рашпилей
Кузнечный молот
Наковальня
Пластина из пьютера4
4
Harden
Harden
Coat the toothed surface thickly with a salt composition against scaling, raise the rasp to a dull red heat in a clear coke fire and plunge it upright into water. If it bends, straighten it across a fulcrum before it is fully cold.
Материалы для этого шага:
Соль1 кг
Металлургический кокс1 as requiredНеобходимые инструменты:
Кузнечный горн
Ведро
Кузнечные клещи5
5
Temper the tang and clean
Temper the tang and clean
Temper the tang by dipping it in molten lead so it will not snap. Scour and wash off every trace of salt, then brush the rasp with oil.
Необходимые инструменты:
Ванна с расплавленным свинцом
Кузнечные клещиМатериалы
3- Заполнитель
- 1 кгЗаполнитель
- 1 as requiredЗаполнитель
Требуемые инструменты
9- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
По этому чертежу делают
Связанные чертежи
Эти чертежи делятся знаниями — техники, материалы или принципы
CC0 Общественное достояние
Этот чертёж выпущен под лицензией CC0. Вы можете свободно копировать, изменять, распространять и использовать эту работу в любых целях без запроса разрешения.
Поддержите мейкера, покупая товары через его чертёж, где он получает Комиссию мейкера установленную продавцами, или создайте новую итерацию этого чертежа и включите его как связь в свой чертёж для распределения дохода.