Black Cobbler's Wax: Resin and Pitch With Linseed Oil, Pulled to Golden Colour (Hasluck, Harness Making, 1904)
The saddler's black wax for waxed threads, from P. N. Hasluck's Harness Making (1904): half a pound each of resin and pitch melted together, softened with boiled linseed oil to suit the season, poured into cold water and pulled by wet hands until golden and until a piece floats. It makes about thirty lumps, kept under water.
Начинающий
About 1 hour
Инструкции
1
1
Batch in grams
Batch in grams
Загрузка блокнота Jupyter…
2
2
Read Harness Making
Read Harness Making
"Black cobbler's wax is made by melting together 1/2 lb. each of resin and pitch."
3
3
Melt and oil
Melt and oil
Melt 1/2 lb of resin and 1/2 lb of pitch together and mix thoroughly. Take the pan off the fire and add boiled linseed oil, about a pennyworth or less: only half as much in summer as in winter, more the colder it is. Mix well.
Материалы для этого шага:
Сосновая смола1 штука
Древесный дёгтевый пек1 штука
Варёное льняное масло1 штукаНеобходимые инструменты:
Большая кастрюля
Пропановая горелка
Рычажные весы4
4
Test
Test
Pour a little into cold water, leave it a minute, and take it out with well-wetted hands. If it cracks when worked it is too hard; if it pulls out and sticks together it is right. Do not put the tested piece back in the pan: the water in it froths the hot wax.
Необходимые инструменты:
Ведро на 20 литров5
5
Pour and pull
Pour and pull
Put the test piece back in the water and pour the rest in after it. Gather the wax with wet hands without delay and pull it fast, hand over hand, until it is a light golden colour. Cut off a piece with wet scissors and drop it in the water: if it floats it has been pulled enough; if it sinks, pull more. Under-pulled wax is brittle.
Необходимые инструменты:
Ведро на 20 литров
Ножницы6
6
Adjust and store
Adjust and store
If it is too hard, melt again and add oil; if too soft, add pitch and resin. Cut it into lumps the size of a large pigeon's egg (about thirty) and keep them in water.
Необходимые инструменты:
Ножницы
Ведро на 20 литров7
7
Troubleshooting
Troubleshooting
Wax troubleshooting.
Flow
Loading...
8
8
History and honest limits
History and honest limits
From Paul N. Hasluck, **Harness Making** (1904), "Harness-makers' Materials" (checked on the archive.org scan harnessmaking00hasl, pp. 30-31). He says only "pitch"; wood-tar pitch is our choice. His white wax, made with white lead, is left out because white lead is a poison. The metric figures and the diagram are ours.
Материалы
3- 1 штукаЗаполнитель
- 1 штукаЗаполнитель
- 1 штукаЗаполнитель
По этому чертежу делают
Связанные чертежи
Эти чертежи делятся знаниями — техники, материалы или принципы
CC0 Общественное достояние
Этот чертёж выпущен под лицензией CC0. Вы можете свободно копировать, изменять, распространять и использовать эту работу в любых целях без запроса разрешения.
Поддержите мейкера, покупая товары через его чертёж, где он получает Комиссию мейкера установленную продавцами, или создайте новую итерацию этого чертежа и включите его как связь в свой чертёж для распределения дохода.