Oriented Barium Ferrite Disc Magnet: Binder Dried in a 2400 Oersted Field (Gorter, Philips 1956, Ex. 3)
A ceramic magnet from pre-fired barium ferrite in polyvinyl acetate and acetone, dried in a 2400 oersted field, then pressed, heated and sintered as in Example 2. In the principal direction it held 2,720 gauss with a coercive force of 1,620 oersted and a (BH)max of 1.2 × 10⁶; at right angles 1,610 gauss.
Source: E. W. Gorter, G. W. Rathenau and A. L. Stuyts (Philips), US 2,762,778 (1956), Example 3. They made blocks; disc size is ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Продвинутый
3 days
Инструкции
1
1
Weigh barium carbonate and iron oxide
Weigh barium carbonate and iron oxide
Weigh 450 g barium carbonate and 2000 g ferric oxide. Barium carbonate is poisonous if swallowed: gloves and a dust respirator.
Материалы для этого шага:
Карбонат бария (витерит)450 г
Оксид железа(III)2000 гНеобходимые инструменты:
Рычажные весы
Резиновые перчатки
Респиратор P1002
2
Mill 20 hours under alcohol, dry
Mill 20 hours under alcohol, dry
Grind the mixture in a ball mill under alcohol for 20 hours, then dry it.
Необходимые инструменты:
Железная шаровая мельница
Этанол - лабораторной чистоты, 95 %
Сушильная печь3
3
Pre-fire: through a 1100 °C zone in 10 minutes
Pre-fire: through a 1100 °C zone in 10 minutes
Pass the dry powder at 20 mm per minute through an electric furnace with a 20 cm hot zone at 1100 °C, in air: 10 minutes in the heat. Let it cool.
Необходимые инструменты:
Трубчатая печь
Тигель с крышкой (фарфоровый)
Термостойкие перчатки4
4
Grind 12 hours with alcohol, dry
Grind 12 hours with alcohol, dry
Pulverise the pre-fired material in a ball mill with alcohol for 12 hours, then dry it. This is the pre-fired powder.
Необходимые инструменты:
Железная шаровая мельница
Этанол - лабораторной чистоты, 95 %
Сушильная печь5
5
Stir into 8 % polyvinyl acetate in acetone
Stir into 8 % polyvinyl acetate in acetone
Dissolve polyvinyl acetate in acetone to a 8 % solution and stir the pre-fired powder into it, 2 cc of solution per gram of powder. The binder burns off later.
Необходимые инструменты:
Поливинилацетат
Ацетон
Рычажные весы6
6
Orient in a 2400 oersted field
Orient in a 2400 oersted field
Put the suspension in a moulding die between the poles of a magnet and apply a first field of 2400 oersted. Remove the binder solution while the field is on.
Необходимые инструменты:
Пресс-форма для дисков
Электромагнит
Гидравлический пресс7
7
Compress into a block
Compress into a block
Compress the powder into a block as in Example 2. The pressure is not given.
Необходимые инструменты:
Гидравлический пресс
Пресс-форма для дисков8
8
Heat to 500 °C in a 2000 oersted field
Heat to 500 °C in a 2000 oersted field
Put the block in an electric furnace between the magnet's poles. With a second field of 2000 oersted along the first field's direction, heat to 500 °C, which burns off the rest of the binder. Then switch the field off.
Необходимые инструменты:
Трубчатая печь
Электромагнит
Термостойкие перчатки9
9
Sinter: through a 1300 °C zone in 5 minutes
Sinter: through a 1300 °C zone in 5 minutes
Pass the block at 20 mm per minute through an electric furnace in air at 1300 °C with a 10 cm hot zone: about 5 minutes in the heat.
Необходимые инструменты:
Трубчатая печь
Термостойкие перчатки10
10
Magnetise in the principal direction
Magnetise in the principal direction
Magnetise the block along the direction of the first field, the principal direction. The patent magnetises it in a field in that direction; ours: an electromagnet. Find the north face with a compass.
Необходимые инструменты:
Электромагнит
КомпасМатериалы
2- Заполнитель
- 2000 гЗаполнитель
Требуемые инструменты
15- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
По этому чертежу делают
Связанные чертежи
Эти чертежи делятся знаниями — техники, материалы или принципы
CC0 Общественное достояние
Этот чертёж выпущен под лицензией CC0. Вы можете свободно копировать, изменять, распространять и использовать эту работу в любых целях без запроса разрешения.
Поддержите мейкера, покупая товары через его чертёж, где он получает Комиссию мейкера установленную продавцами, или создайте новую итерацию этого чертежа и включите его как связь в свой чертёж для распределения дохода.