Phthalic Anhydride by Air Oxidation of Naphthalene: Gibbs and Conover, 1918
Charlie

Создано

Charlie

13. октябрь 2026DE
15
0
0
0
0

Phthalic Anhydride by Air Oxidation of Naphthalene: Gibbs and Conover, 1918

Harry D. Gibbs and Courtney Conover patented this in 1918, US 1,285,117 (filed 1917), and dedicated it to the public. Phthalic anhydride had been made by oxidising naphthalene with sulphuric acid in the presence of mercury sulphate; they used air instead. Naphthalene vapour mixed with plenty of air is passed over finely divided oxides of vanadium at 350–550 °C, and the phthalic anhydride formed is condensed and separated by fractional sublimation.
Продвинутый
Works process

Инструкции

1

Melt and vaporise the naphthalene

Melt the naphthalene and let it flow continuously, at a measured rate, into a heated chamber where it is volatilised.

Материалы для этого шага:

НафталинНафталин1 as required

Необходимые инструменты:

Чугунный тигельЧугунный тигель
Испарительная камераИспарительная камера
ТермометрТермометр
2

Mix the vapour with air

Mix the naphthalene vapour with air in excess of the amount needed to oxidise it to phthalic anhydride, preferably at least four times the amount theoretically required.

Необходимые инструменты:

ВоздуходувкаВоздуходувка
Испарительная камераИспарительная камера
3

Pass it over vanadium oxide at 350–550 °C

Pass the mixture into a reaction chamber kept at 350–550 °C, preferably 500 °C. There it is forced into close contact with oxides of vanadium in the form of a fine powder, supported on trays, with baffle plates forcing the gas current through it. Keep the gases under pressure only sufficient to make them flow continuously through the chamber. The naphthalene is oxidised to phthalic anhydride, with carbon dioxide and water.

Необходимые инструменты:

Каталитическая камера с полкамиКаталитическая камера с полками
Оксид ванадияОксид ванадия
ПирометрПирометр
ВоздуходувкаВоздуходувка
4

Condense the products

Condense the products of the reaction, phthalic anhydride with small portions of other oxidation products of naphthalene, together with the unchanged naphthalene.

Необходимые инструменты:

Конденсационная камераКонденсационная камера
5

Separate by fractional sublimation

Separate the phthalic anhydride from the other oxidation products and the unchanged naphthalene by fractional sublimation.

Необходимые инструменты:

Аппарат для возгонкиАппарат для возгонки
ТермометрТермометр
6

How much air

Загрузка блокнота Jupyter…

Материалы

1
  • 1 as required
    Заполнитель

Требуемые инструменты

9

По этому чертежу делают

Связанные чертежи

Эти чертежи делятся знаниями — техники, материалы или принципы

CC0 Общественное достояние

Этот чертёж выпущен под лицензией CC0. Вы можете свободно копировать, изменять, распространять и использовать эту работу в любых целях без запроса разрешения.

Поддержите мейкера, покупая товары через его чертёж, где он получает Комиссию мейкера установленную продавцами, или создайте новую итерацию этого чертежа и включите его как связь в свой чертёж для распределения дохода.

Обсуждение

(0)

Войти чтобы присоединиться к обсуждению

Загрузка комментариев...