Porcelain Labware: Evaporating Dishes, Crucibles, Funnels and Streak Plates
Hard porcelain stands strong heat and most chemicals, so the laboratory's dishes, crucibles and filter funnels are made of it; left unglazed, its white biscuit is the streak plate for testing minerals. Form the pieces, give them a light first firing, dip them in ground-felspar glaze, and fire them hard in saggers, as Andrew Ure (1839) describes for Sèvres.
The picture: porcelain evaporating dishes in three sizes, glazed, with pouring lips.
Продвинутый
Weeks with drying and two firings
Инструкции
1
1
Form the pieces
Form the pieces
Throw shallow round dishes with a lip and small lidded crucibles on the wheel. For a Büchner funnel throw a cylinder with a flat floor, pierce the floor with many small holes and add a stem. Roll a slab and cut it into small tiles for streak plates.
Материалы для этого шага:
Фарфоровая масса5 кгНеобходимые инструменты:
Гончарный круг
Скалка
Набор гончарных инструментов
Линейка2
2
Dry very slowly
Dry very slowly
Ure: dry them very slowly; a little hurry spoils them.
3
3
Light first firing
Light first firing
Fire them gently so they keep their shape but become strong enough to handle and be dipped in water.
Материалы для этого шага:
Дрова1 as requiredНеобходимые инструменты:
Печь для обжига
Термостойкие перчатки4
4
Felspar glaze
Felspar glaze
Grind felspar very fine, stir it with water and a little vinegar to a thin pap. Dip each dish, crucible and funnel for an instant; the porous body draws the glaze on. Wipe the glaze off the feet. Leave the streak-plate tiles unglazed.
Материалы для этого шага:
Кусок полевого шпата0.5 кг
Вода2 литров
Уксус0.05 литрНеобходимые инструменты:
Курант
Сито с мелкой сеткой
Чан
Противопылевая маска5
5
Set in saggers
Set in saggers
Set every piece in its own sagger on a flat, sand-dusted base so it cannot stick or sag out of shape; small pieces may share a base if they do not touch.
Материалы для этого шага:
Мелкий песок1 кгНеобходимые инструменты:
Капсель6
6
The hard firing
The hard firing
Raise the fire slowly for about 15 hours to a cherry red, then fire hard until the kiln glows white inside, drawing trial pieces to judge when the glaze is smooth. Cool slowly over days.
Материалы для этого шага:
Дрова1 as requiredНеобходимые инструменты:
Печь для обжига
Термостойкие перчатки7
7
Ure's firing, hour by hour
Ure's firing, hour by hour
Загрузка блокнота Jupyter…
8
8
Limits
Limits
The firings, glaze and saggers are Ure's account of Sèvres; the forms of the four wares are ours. A full porcelain firing needs a kiln that reaches white heat.
Материалы
6- 5 кгЗаполнитель
- 1 as requiredЗаполнитель
- 0.5 кгЗаполнитель
- 2 литровЗаполнитель
- 0.05 литрЗаполнитель
- 1 кгЗаполнитель
Требуемые инструменты
11- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
- Заполнитель
По этому чертежу делают
Связанные чертежи
Эти чертежи делятся знаниями — техники, материалы или принципы
CC0 Общественное достояние
Этот чертёж выпущен под лицензией CC0. Вы можете свободно копировать, изменять, распространять и использовать эту работу в любых целях без запроса разрешения.
Поддержите мейкера, покупая товары через его чертёж, где он получает Комиссию мейкера установленную продавцами, или создайте новую итерацию этого чертежа и включите его как связь в свой чертёж для распределения дохода.