Strontium Ferrite Disc Magnet: 0.7 mol SrCO3 to 3.2 mol Iron Oxide, 1280 °C (Went, Philips 1956, Ex. 12)
Charlie

Создано

Charlie

28. октябрь 2026DE
9
0
0
0
0

Strontium Ferrite Disc Magnet: 0.7 mol SrCO3 to 3.2 mol Iron Oxide, 1280 °C (Went, Philips 1956, Ex. 12)

A strontium ferrite: 0.7 mol strontium carbonate to 3.2 mol iron oxide, milled, bound and formed as in Example 4, and passed through a 1280 °C furnace in 10 minutes. Went's rod held 1,955 gauss with a coercive force of 2,900 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956), Example 12. They sintered rods; discs and the magnetising are ours. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Продвинутый
2 days

Инструкции

1

Weigh strontium carbonate and iron oxide

Weigh 103.3 g strontium carbonate (0.7 mol) and 503.0 g ferric oxide (3.2 mol).

Материалы для этого шага:

Карбонат стронцияКарбонат стронция103.3 г
Оксид железа(III)Оксид железа(III)503 г

Необходимые инструменты:

Рычажные весыРычажные весы
Респиратор P100Респиратор P100
2

Mill with alcohol 15.5 hours, dry and sieve

As in Example 4: grind the mixture with alcohol in a ball mill for 15.5 hours, then dry it and sieve it.

Необходимые инструменты:

Железная шаровая мельницаЖелезная шаровая мельница
Этанол - лабораторной чистоты, 95 %Этанол - лабораторной чистоты, 95 %
Сушильная печьСушильная печь
ГрохотГрохот
3

Knead with a binder and form

Mix 300 g of the powder with a binder such as polyvinyl alcohol (Went names it or nitrocellulose) into a kneadable mass. The patent extrudes rods about 3 mm across; ours: press discs at 1.5 tonnes per cm², as in its other examples. Dry them in air for about 24 hours.

Необходимые инструменты:

Поливиниловый спирт в порошкеПоливиниловый спирт в порошке
Гидравлический прессГидравлический пресс
Пресс-форма для дисковПресс-форма для дисков
Сушильная печьСушильная печь
4

Pass through a 1280 °C zone in 10 minutes

Sinter in air at 1280 °C by passing the pieces through a 10 cm hot zone at 10 mm per minute: 10 minutes in the heat.

Необходимые инструменты:

Трубчатая печьТрубчатая печь
Термостойкие перчаткиТермостойкие перчатки
5

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Необходимые инструменты:

ЭлектромагнитЭлектромагнит
КомпасКомпас

Материалы

2

Требуемые инструменты

13

По этому чертежу делают

CC0 Общественное достояние

Этот чертёж выпущен под лицензией CC0. Вы можете свободно копировать, изменять, распространять и использовать эту работу в любых целях без запроса разрешения.

Поддержите мейкера, покупая товары через его чертёж, где он получает Комиссию мейкера установленную продавцами, или создайте новую итерацию этого чертежа и включите его как связь в свой чертёж для распределения дохода.

Обсуждение

(0)

Войти чтобы присоединиться к обсуждению

Загрузка комментариев...