Reading a Plating Fault: Burnt, Pitted, Dull, Peeling

Plating faults have distinct appearances, and each one points at a short list of causes. The diagnosis is quicker than the repair, and it is what stops the same batch being ruined twice. The first question is always **where** the fault is. A fault at the edges is a current density problem. A fault in a recess is a throwing power problem. A fault in a patch with a defined shape is contamination — and the shape usually says what it was. A fault over the whole part is the bath.
Hagati
2 hours

Amabwiriza

1

Burning, and roughness

**Burning** is a dark grey, rough, powdery deposit with poor adhesion, always worst at edges, corners and points. It is a dendritic growth: the deposit has grown faster than ions can arrive, so it has branched out into the solution rather than filling in. *Causes, in order:* current density too high — either the current was set too high or the area was underestimated; too little agitation; the bath too cold; the metal concentration too low. *The fix at the edges specifically:* a thief, a shield, or a lower current. The racking rung covers these. **Roughness** is different — gritty or nodular over the whole surface, with good adhesion. It is particles in the bath being plated over. *Causes:* particles falling from the anodes, which is why anodes go in bags; precipitated basic salts from a pH that drifted high; dust; filter failure. *The fix:* filter the bath continuously, bag the anodes, check the pH. **The two are told apart by adhesion and by location.** Burning is at the extremities and lifts; roughness is everywhere and sticks.

Ibikoresho by'iyi ntambwe:

Ikibaho cy'icyuma cyorohejeIkibaho cy'icyuma cyoroheje2 ibice
Sulfate ya nikel ifite amazi atandatuSulfate ya nikel ifite amazi atandatu1 igice

Ibikoresho bikenewe:

Lupu YaguraLupu Yagura
Multimeter ya dijitali — ibipimo byihitamo, RMS nyayoMultimeter ya dijitali — ibipimo byihitamo, RMS nyayo
2

Pitting, and why hydrogen causes it

**Pitting** is small round holes or craters in the deposit, often in trails running upwards, and it has one dominant cause: **a hydrogen bubble stuck to the surface**. Where a bubble sits, no metal deposits, and the deposit grows around it into a pit. The trails happen because the bubble slides upwards as it grows. *Causes and fixes:* **Poor wetting** — the commonest. A wetting agent in the bath lowers the surface tension so bubbles release instead of clinging. Its exhaustion is the usual reason a bath starts pitting after months of working. **Too little agitation** — bubbles are not swept away. **Organic contamination** — oil in the bath, often from a part that was not properly degreased, stabilises the bubbles. Carbon treatment removes it. **Low current efficiency** — more hydrogen produced in the first place, which is why chrome pits so readily. **A horizontal surface facing upwards pits worst**, because bubbles settle on it. Rotating or tilting the work during plating is a genuine fix and costs nothing.

Ibikoresho by'iyi ntambwe:

Ikibaho cy'icyuma cyorohejeIkibaho cy'icyuma cyoroheje2 ibice

Ibikoresho bikenewe:

Lupu YaguraLupu Yagura
Ubuso bushyushya bufite kivanga cya rukuruziUbuso bushyushya bufite kivanga cya rukuruzi
3

Dullness, cloudiness and staining

**Dullness where brightness was expected.** The brightener is exhausted, the current density is below the bright range, the temperature is wrong, or the substrate was not polished — a bright bath does not make a dull surface bright unless it is a levelling bath, and even then only up to a point. **Cloudiness or haze**, especially in low current density areas. Usually organic contamination, and carbon treatment is the answer. **A milky or smutty grey film** that wipes off. Often a metallic contaminant co-depositing — zinc in a nickel bath, for instance. Dummy plating at low current density for several hours removes it onto a scrap cathode. **Staining after drying.** Solution not rinsed out, or a hole that weeped after the part was dry, or tap water in the last rinse. **A rainbow or iridescent sheen on zinc** is the passivation film and is normal — that one is a feature. **Brown or black streaks running down from a hole** are trapped solution finding its way out after plating. Blow the holes out before drying.

Ibikoresho by'iyi ntambwe:

Sulfate ya nikel ifite amazi atandatuSulfate ya nikel ifite amazi atandatu1 igice
Amazi YatunganyijweAmazi Yatunganyijwe1 igice

Ibikoresho bikenewe:

Lupu YaguraLupu Yagura
Igikombe cya BorosilikateIgikombe cya Borosilikate
4

The diagnostic sequence, and the log

**Start with where.** Edges and points say current density. Recesses and blind areas say throwing power. A patch with a shape — a thumb print, a run mark, a line where the solution level sat — says contamination or handling. Everywhere at once says the bath. **Then ask when it started.** A fault that appeared suddenly between two otherwise identical runs points at a single change: a new bottle of something, a topped-up bath, a different part, a colder day. A fault that has crept in over weeks points at consumption — brightener, wetting agent, anode area. **Then run a Hull cell.** One small panel shows the whole current density range at once: where it burns, where it goes dull, where it is bright. It is the single most informative half hour available, and it uses a few hundred millilitres. **Then treat in the standard order:** filter, carbon treat for organics, dummy plate for metallics, correct the pH, correct the temperature, and only then add brightener. Adding brightener first is the usual instinct and it usually makes things worse, because the additive is rarely the cause. **Keep the log.** Date, part, area, current, time, temperature, pH, weight gain, and what the deposit looked like. Every diagnosis above is a comparison against a previous run, and without the log there is nothing to compare with.

Ibikoresho by'iyi ntambwe:

Ikarito yo gusiga icyuma amashanyarazi (nikeli)Ikarito yo gusiga icyuma amashanyarazi (nikeli)1 igice

Ibikoresho bikenewe:

Isoko ry'Amashanyarazi ry'Ameza RihindurwaIsoko ry'Amashanyarazi ry'Ameza Rihindurwa
Multimeter ya dijitali — ibipimo byihitamo, RMS nyayoMultimeter ya dijitali — ibipimo byihitamo, RMS nyayo
Igipima Ubushyuhe cy'UbushakashatsiIgipima Ubushyuhe cy'Ubushakashatsi

Ibikoresho

4

Ibikoresho bikenewe

6

CC0 Umurenge rusange

Iyi blueprint yasohowe munsi ya CC0. Ushobora gukoporora, guhindura, gukwirakwiza no gukoresha nta kwemererwa.

Shyigikira Umuremyi ugura ibicuruzwa binyuze muri Blueprint ye Komisiyo y'Umuremyi byashyizweho n'Abacuruzi, cyangwa kora verisiyo nshya y'iyi Blueprint ukayinjiza nk'isano muri Blueprint yawe kugira ngo musangire inyungu.

Ibiganiro

(0)

Injira kugira ngo ujye mu biganiro

Gutegura ibitekerezo...