Neodymium Magnets, Sample 2: 83Fe-2B-15Nd Sintered (Sagawa 1988)
Neodymium magnets are iron, boron and neodymium. Sagawa's team at Sumitomo melted the three together, ground the casting to a powder finer than 10 µm, lined the grains up in a magnetic field while pressing them, and sintered the compact in argon. This is their sample 2, 83 % iron, 2 % boron and 15 % neodymium by atoms: 4.1 MGOe.
Source: M. Sagawa et al. (Sumitomo Special Metals), US 4,770,723 (1988). Unknown: how the pure iron, the ferroboron and the neodymium metal are made; the patent does not say. The magnetising is ours, after Przybylski et al., Sensors 16:569 (2016). The 1 kg weights are our arithmetic from the patent's atomic percentages. Picture: the patent's Fig. 8.
Impuguke
2 days
Amabwiriza
1
1
Weigh sample 2: 83 Fe, 2 B, 15 Nd
Weigh sample 2: 83 Fe, 2 B, 15 Nd
Sample 2 is 83 % iron, 2 % boron and 15 % neodymium by atoms. Use 99.9 % electrolytic iron, ferroboron (19.38 % B, 5.32 % Al, 0.74 % Si, 0.03 % C, the rest iron) and neodymium of 99.7 % or better. Ours: a 1 kg melt, by arithmetic: 667.4 g iron, 16.4 g ferroboron, 317.2 g neodymium. Unknown: how these three are made.
Ibikoresho by'iyi ntambwe:
Icyuma cyo mu mashanyarazi667.4 g
Ferroboron16.4 g
Icyuma cya neodymium317.2 gIbikoresho bikenewe:
Umunzani w'ibiro2
2
Melt by high frequency in argon and cast
Melt by high frequency in argon and cast
Melt the charge in a high-frequency (induction) furnace under argon and pour it into a water-cooled copper mould.
Ibikoresho bikenewe:
Itanura rya induction
Ikirahure cy'Ibumba Rirwanya Umuriro
Arigoni
Ibariro rya gazi ifite igitutu
Ifumbiro ry’umuringa rikonjeshwa n’amazi
Uturindantoki twihanganira ubushyuhe3
3
Stamp to 35 mesh, ball-mill to 3-10 µm
Stamp to 35 mesh, ball-mill to 3-10 µm
Crush the casting in a stamp mill until it passes a 35-mesh sieve. Then grind it in a ball mill for 3 hours, to 3-10 µm.
Ibikoresho bikenewe:
Imashini Ikoma Amabuye
Agatsiko k'utuyungurizo (imyobo itandukanye)
Urusyo rw'imipira y'icyuma
Amadarubindi y'umutekano4
4
Press in a 10 kOe field at 1.5 t/cm²
Press in a 10 kOe field at 1.5 t/cm²
Line the powder up in a magnetic field of 10 kOe and press it at 1.5 tonnes per cm². Unknown: the size and shape of the magnets.
Ibikoresho bikenewe:
Imashini ikanda ifite umurima wa rukuruzi5
5
Sinter in argon at 1000-1200 °C
Sinter in argon at 1000-1200 °C
Sinter the compacts at 1000-1200 °C for about one hour in argon, then let them cool. Sample 2 measured 7.5 kG remanence, 1.3 kOe coercivity and 4.1 MGOe.
Ibikoresho bikenewe:
Itanura ry'umuyoboro
Arigoni
Ibariro rya gazi ifite igitutu
Uturindantoki twihanganira ubushyuhe6
6
Magnetise the magnets
Magnetise the magnets
Ours, after Przybylski et al., Sensors 16:569 (2016): put each magnet in the coil of an impulse magnetiser and discharge a capacitor bank through it. They found a field of 1200 kA/m enough to saturate N38 sintered Nd-Fe-B; their magnetiser used a 1 mF bank charged up to 5000 V, a thyristor switch and a 440-turn coil of 3 mm copper wire with an 80 mm bore.
Ibikoresho bikenewe:
Imashini itera rukuruziIbikoresho
3- 667.4 gUmwanya
- 16.4 gUmwanya
- 317.2 gUmwanya
Ibikoresho bikenewe
14- Umwanya
- Umwanya
- Umwanya
- Umwanya
- Umwanya
- Umwanya
- Umwanya
- Umwanya
Iki gishushanyo gikora
Blueprint zijyanye
Izi blueprint zisangira ubumenyi — uburyo, ibikoresho cyangwa amahame
CC0 Umurenge rusange
Iyi blueprint yasohowe munsi ya CC0. Ushobora gukoporora, guhindura, gukwirakwiza no gukoresha nta kwemererwa.
Shyigikira Umuremyi ugura ibicuruzwa binyuze muri Blueprint ye Komisiyo y'Umuremyi byashyizweho n'Abacuruzi, cyangwa kora verisiyo nshya y'iyi Blueprint ukayinjiza nk'isano muri Blueprint yawe kugira ngo musangire inyungu.