Zinc Powder: Zinc Crushed Hot, Just Below Melting
Zinc has an odd temper: brittle cold, soft enough to roll at 100 to 150 °C, and above 200 °C so tender that it crushes to powder. Thorpe (1913): zinc dust can be made by crushing the metal in a mortar at a heat somewhat below its melting point of 420 °C. Work hot with leather gloves.
The picture: our own drawing.
Utangiye
Half a day
Amabwiriza
1
1
Cut the zinc small
Cut the zinc small
Saw 300 g of zinc into small pieces.
Ibikoresho by'iyi ntambwe:
Ikibumbe cya zenke300 gIbikoresho bikenewe:
Umucumita w'Ibyuma
Umunzani w'ibiro2
2
Heat to just below melting
Heat to just below melting
Heat the pieces in an iron pot above 200 °C but below 420 °C, where zinc melts. Check with a pyrometer.
Ibikoresho bikenewe:
Inkono y'icyuma cyasuwe
Iziko ry'amakara
Pirometero
Uturindantoki tw'Uruhu3
3
Crush in the mortar
Crush in the mortar
Tip a few hot pieces at a time into the mortar and crush them. Hot zinc breaks to powder; reheat what is left whole.
Ibikoresho bikenewe:
Isekuru n'Umuhini
Uturindantoki tw'Uruhu4
4
Sieve and store
Sieve and store
Sieve the cooled powder, return the coarse bits for another crushing, and keep the powder in a closed jar.
Ibikoresho bikenewe:
Ishungura rito
Icupa ry'Ikirahure Rifite UmufunikoIbikoresho
1- 300 gUmwanya
Ibikoresho bikenewe
9- Umwanya
- Umwanya
- Umwanya
- Umwanya
- Umwanya
- Umwanya
- Umwanya
- Umwanya
Iki gishushanyo gikora
CC0 Umurenge rusange
Iyi blueprint yasohowe munsi ya CC0. Ushobora gukoporora, guhindura, gukwirakwiza no gukoresha nta kwemererwa.
Shyigikira Umuremyi ugura ibicuruzwa binyuze muri Blueprint ye Komisiyo y'Umuremyi byashyizweho n'Abacuruzi, cyangwa kora verisiyo nshya y'iyi Blueprint ukayinjiza nk'isano muri Blueprint yawe kugira ngo musangire inyungu.