Current Density: Edges Plate Thick and Recesses Do Not Plate At All

Faraday's law says how much metal is deposited. It says nothing about where it goes, and the answer is: not evenly. Current takes the shortest path through the solution, so the parts of the work nearest the anode get more of it, and edges, corners and points — which current can reach from several directions at once — get the most. Recesses and the insides of tubes may get almost none. **Throwing power** is how well a particular bath evens this out, and it varies enormously between chemistries. Understanding it is the difference between a part that is plated and a part that is plated on the side that faced the anode.
متقدم
4 hours

التعليمات

1

Current density is the specification, not current

Every plating bath is specified in **amps per square decimetre** of cathode area, and 1 dm² is 100 cm², which is a convenient size of part. **So the area must be calculated before the current is set.** Both faces, the edges, and the inside of any hole. A part whose area is underestimated is plated at a higher current density than intended, and the symptom is burning at the edges. **Below the window:** a dull, thin, sometimes non-existent deposit. Some baths will not deposit at all below a threshold current density, so a part with a deep recess can be plated everywhere except inside it — not thinly, but not at all. **Above the window:** **burning**. A dark grey, rough, powdery deposit with little adhesion, always worst at edges and points. It cannot be polished out; the part is stripped and started again. **The window moves with temperature and agitation.** Both allow higher current density, because both bring fresh solution to the cathode faster. A bath run cold at its normal current burns; the same bath hot and stirred does not. **Start low.** A part plated slowly at the bottom of the window is right; one plated fast at the top is a gamble on the area calculation.

المواد لهذه الخطوة:

لوح صلب طريلوح صلب طري2 قطع
كبريتات النيكل سداسية الماءكبريتات النيكل سداسية الماء1 قطعة

الأدوات المطلوبة:

مصدر تغذية مختبري قابل للضبطمصدر تغذية مختبري قابل للضبط
مقياس متعدّد رقمي — تدرّج تلقائي، RMS حقيقيمقياس متعدّد رقمي — تدرّج تلقائي، RMS حقيقي
قدمة رقمية 6 بوصاتقدمة رقمية 6 بوصات
2

Where the metal goes, and which baths spread it

جارٍ تحميل دفتر Jupyter…

الأدوات المطلوبة:

حاسوب مكتبيحاسوب مكتبي
3

Racking, thieves and shields

How the work hangs in the tank is a real part of the process, and there are four standard tools. **Racking.** Every part hangs from a rack that carries current to it. The contact must be firm and must be somewhere that does not matter, because the contact point does not plate and often leaves a mark. Hang parts so that air cannot be trapped in a recess — a trapped bubble is an unplated patch with a sharp edge. **Orientation.** Present the important face to the anode. A part hung edge-on to the anode plates its edges and starves its faces. **Thieves** (robbers). A sacrificial piece of metal placed near an edge or a corner, which takes the excess current instead of the part. It is the standard answer to burning at one specific feature, and it costs a scrap of metal. **Shields.** A non-conducting barrier — plastic sheet — placed between the anode and a part of the work that would otherwise get too much current. The opposite of a thief, and used where a thief would be in the way. **Conforming and auxiliary anodes.** For an awkward shape, an anode shaped to follow the part, or a small anode placed inside a recess. This is how the inside of a tube or the bore of a cylinder is hard-chromed, and it is essentially the only way. **Barrel plating** tumbles many small parts in a perforated barrel, so each one spends time at every position. The distribution problem is solved by moving the parts rather than the current.

المواد لهذه الخطوة:

لوح صلب طريلوح صلب طري2 قطع
صفيحة نحاسصفيحة نحاس1 قطعة

الأدوات المطلوبة:

مصدر تغذية مختبري قابل للضبطمصدر تغذية مختبري قابل للضبط
كأس زجاج بوروسيليكاتيكأس زجاج بوروسيليكاتي
شريط لاصق ورقيشريط لاصق ورقي
4

Masking and selective plating

Sometimes the answer is to plate only part of the work. **Lacquer or stop-off paint.** A peelable or solvent-removable coating painted on the areas not to be plated. It must resist the bath chemistry, which for an acid bath and an alkaline bath are different requirements. **Plating tape.** Chemically resistant adhesive tape, cut to shape. Fast, accurate at an edge, and it lifts if the surface was not properly clean — which is a useful early warning. **Wax.** The traditional stop-off, still good for an irregular shape, and it melts off cleanly afterwards. **Mechanical masks.** A plug in a threaded hole, a cap over a bearing surface. Reusable and precise for production. **Brush plating** goes the other way: no tank at all. An anode wrapped in an absorbent pad soaked in concentrated solution is stroked over the work with current flowing. It plates exactly where the pad touches, it is how worn machinery is repaired in place, and it works at very high current densities because the pad brings fresh solution constantly. **Whatever the mask, the edge of it is a weak point.** The coating is at its thinnest where it meets the mask, and that is where corrosion starts. Put the boundary where it will not matter.

المواد لهذه الخطوة:

شريط لاصق ورقيشريط لاصق ورقي1 قطعة
لوح صلب طريلوح صلب طري1 قطعة

الأدوات المطلوبة:

مصدر تغذية مختبري قابل للضبطمصدر تغذية مختبري قابل للضبط
قفازات مقاومة للكيماوياتقفازات مقاومة للكيماويات

المواد

4

الأدوات المطلوبة

7

المخططات ذات الصلة

هذه المخططات تشارك المعرفة مع هذا — التقنيات والمواد والمبادئ

CC0 ملكية عامة

هذا المخطط مُصدر بموجب CC0. يحق لك نسخه وتعديله وتوزيعه واستخدامه لأي غرض، دون طلب إذن.

ادعم الصانع بشراء منتجات عبر مخططه حيث يكسب عمولة الصانع يحددها البائعون، أو أنشئ نسخة جديدة من هذا المخطط وضمّنه كرابط في مخططك لمشاركة الإيرادات.

النقاش

(0)

تسجيل الدخول للمشاركة في النقاش

جارٍ تحميل التعليقات...