Ebonite (Hard Rubber)
Vulcanised rubber is rubber with a few sulphur bridges between its chains. Keep adding sulphur and the bridges multiply until the chains cannot move at all: the soft, stretchy material turns into a hard black solid you can turn on a lathe, polish like ebony and use as an electrical insulator.
**US 8,075**, "Improvement in the Manufacture of India Rubber", Nelson Goodyear (brother of Charles), granted 6. May 1851, claims "the combining of india-rubber and sulphur… for making a hard and inflexible substance hitherto unknown": about equal parts by weight, heated to 260–275 °F for three to six hours. It was one of the first rigid materials made by chemically changing a natural polymer, over half a century before Bakelite.
**You turn a part from commercial ebonite rod and measure what the sulphur did** — its density, and its charge when rubbed. Curing ebonite needs a heated press and releases hydrogen sulphide, so the blueprint starts from finished rod; the notebook does the chemistry.
متوسط
3 hours
التعليمات
1
1
Cut the blank
Cut the blank
Clamp 20 mm ebonite rod in the vise between soft jaws. Saw off 60 mm. Ebonite chips like hard wood; saw slowly to avoid cracking the end.
المواد لهذه الخطوة:
قضيب إيبونيت1 قطعةالأدوات المطلوبة:
منشار حديد
ملزمة منضدة
مسطرة فولاذية
نظارة أمان شفافة2
2
Chuck and face
Chuck and face
Grip 20 mm of the blank in the lathe's 3-jaw chuck. Face the end square with a sharp HSS tool at about 800 rpm, light cuts.
الأدوات المطلوبة:
مخرطة معادن
طقم أدوات المخرطة (HSS)
نظارة أمان شفافة
كمامة غبار3
3
Turn to 16 mm
Turn to 16 mm
Turn 40 mm of length down to 16.0 mm. Check with the caliper every pass. The chips smell of sulphur - that is the bonded sulphur you measure later.
الأدوات المطلوبة:
مخرطة معادن
طقم أدوات المخرطة (HSS)
قدمة رقمية 6 بوصات4
4
Drill the bore
Drill the bore
Spot the centre with a centre drill, then drill 3 mm through 35 mm from the tailstock. Clear chips every 5 mm - ebonite heats and gums if packed.
الأدوات المطلوبة:
طقم مثاقب تنقيط
طقم لُقم ثقب في علبة
مخرطة معادن5
5
Taper the grip
Taper the grip
Set the compound to a shallow angle and taper 25 mm from 16 mm down to 10 mm. This is a fountain-pen grip section, the job ebonite still does today.
الأدوات المطلوبة:
مخرطة معادن
طقم أدوات المخرطة (HSS)
قدمة رقمية 6 بوصات6
6
Sand and polish
Sand and polish
At low speed, sand 400 then 800 grit, then run the Micro-Mesh grits in order. Finish with polishing compound on a cloth. Ebonite takes a deep gloss without lacquer.
المواد لهذه الخطوة:
ورق صنفرة2 أوراق
معجون تلميع5 غالأدوات المطلوبة:
طقم صنفرة بالشبكة الدقيقة (9 خشونات)
مخرطة معادن
كمامة غبار7
7
Part off
Part off
Part off at 45 mm with the parting tool. Chamfer the cut end by hand with 800 grit.
الأدوات المطلوبة:
طقم أدوات المخرطة (HSS)
مخرطة معادن8
8
Measure the density
Measure the density
Weigh the part. Drop it into 50 ml of water in the graduated cylinder and read the rise. Do the same with a bundle of rubber bands. Enter both in the notebook.
المواد لهذه الخطوة:
أربطة مطاطية1 عبوةالأدوات المطلوبة:
ميزان رقمي دقيق
مخبار مدرّج9
9
Rub it and pick up paper
Rub it and pick up paper
Tear tissue into 5 mm scraps. Rub the ebonite 10 strokes on wool felt and hold it 2 cm above the scraps. Repeat with an acrylic offcut. Count scraps lifted by each.
المواد لهذه الخطوة:
ورق حرير خالٍ من الحمض1 ورقة
لوح أكريليك1 قطعةالأدوات المطلوبة:
لبّاد صوفي10
10
The sulphur arithmetic
The sulphur arithmetic
جارٍ تحميل دفتر Jupyter…
11
11
History & Context
History & Context
**What the patent specifies:** rubber and sulphur in about equal parts (or 2 : 1 with magnesia or lime), 260–275 °F, three to six hours. **Modern build (derived):** commercial ebonite rod, typically 25–32 % sulphur - the notebook shows why more than about 32 % cannot bond.
Ebonite was named for ebony, which it replaced in combs, pipe stems and instrument parts. It became a standard insulator of the electrical age and is still preferred for fountain-pen feeds because ink wets it. Its limits: it softens with heat, fades to brown and smells of sulphur in sunlight as the surface oxidises, and is brittle under impact.
المواد
6- 1 قطعةعنصر نائب
- 2 أوراقعنصر نائب
- 5 غعنصر نائب
- 1 عبوةعنصر نائب
- 1 ورقةعنصر نائب
- 1 قطعةعنصر نائب
الأدوات المطلوبة
14- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- طقم مثاقب تنقيطعمولة 10%عنصر نائب
- عنصر نائب
- طقم صنفرة بالشبكة الدقيقة (9 خشونات)عمولة 10%عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
المخططات ذات الصلة
هذه المخططات تشارك المعرفة مع هذا — التقنيات والمواد والمبادئ
CC0 ملكية عامة
هذا المخطط مُصدر بموجب CC0. يحق لك نسخه وتعديله وتوزيعه واستخدامه لأي غرض، دون طلب إذن.
ادعم الصانع بشراء منتجات عبر مخططه حيث يكسب عمولة الصانع يحددها البائعون، أو أنشئ نسخة جديدة من هذا المخطط وضمّنه كرابط في مخططك لمشاركة الإيرادات.