Methyl Methacrylate Syrup: Partly Polymerised below 80 °C with Hydrogen Peroxide
Methyl methacrylate syrup is the monomer partly polymerised until it is thick: the stock that is poured between glass plates to cast acrylic sheet. ICI's Tattersall (US 2,071,907, 1937) heats the liquid monomer with a little catalyst, never above 80 °C, until it is syrupy, then cools it. His example used benzoyl peroxide and he names hydrogen peroxide as an alternative but gives no amount. Our choice: 14 g of 3 % hydrogen peroxide per kg of monomer, as many peroxide molecules as his 0.3 % benzoyl peroxide. Methyl methacrylate is flammable: no open flame.
The picture: our diagram.
متوسط
Half a day
التعليمات
1
1
Weigh monomer and peroxide
Weigh monomer and peroxide
Weigh liquid methyl methacrylate into a round-bottom flask and add 14 g of 3 % hydrogen peroxide per kg of monomer (our amount; the patent only says a relatively small amount).
المواد لهذه الخطوة:
ميثاكريلات الميثيل1 كغ
بيروكسيد الهيدروجين (3 %)14 غالأدوات المطلوبة:
دورق كروي القاع
ميزان ذو كفّتين
نظارة واقية من رذاذ الكيماويات
قفازات مطاطية
خزانة أبخرة (بمجرى تصريف)2
2
Heat, never above 80 °C
Heat, never above 80 °C
Fit a reflux condenser and warm the flask in a water bath to near but not above 80 °C. Above 80 °C the finished sheet is not flawless; lower temperatures work but take longer.
الأدوات المطلوبة:
دورق كروي القاع
مكثف الارتجاع
حمام مائي
صفيحة تسخين
ميزان حرارة مختبري
خزانة أبخرة (بمجرى تصريف)3
3
Stop when it is syrupy
Stop when it is syrupy
Check the thickness now and then with a glass rod. Stop when the liquid has become a syrup. The patent took its example to a molecular weight of 3000, measured by viscosity, and gives no time.
الأدوات المطلوبة:
قضيب تحريك زجاجي
ميزان حرارة مختبري4
4
Cool to room temperature
Cool to room temperature
Cool the syrup to about room temperature (30 °C in the example) in cold water. It is then ready to pour between glass plates and cast into sheet.
الأدوات المطلوبة:
حوض تبريد مائي
ميزان حرارة مختبري
قفازات مطاطيةالمواد
2- عنصر نائب
- عنصر نائب
الأدوات المطلوبة
11- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
هذا المخطط يصنع
المخططات ذات الصلة
هذه المخططات تشارك المعرفة مع هذا — التقنيات والمواد والمبادئ
CC0 ملكية عامة
هذا المخطط مُصدر بموجب CC0. يحق لك نسخه وتعديله وتوزيعه واستخدامه لأي غرض، دون طلب إذن.
ادعم الصانع بشراء منتجات عبر مخططه حيث يكسب عمولة الصانع يحددها البائعون، أو أنشئ نسخة جديدة من هذا المخطط وضمّنه كرابط في مخططك لمشاركة الإيرادات.