Neodymium Magnets, Sample 8: 75Fe-10B-15Nd Sintered (Sagawa 1988)
Neodymium magnets are iron, boron and neodymium. Sagawa's team at Sumitomo melted the three together, ground the casting to a powder finer than 10 µm, lined the grains up in a magnetic field while pressing them, and sintered the compact in argon. This is their sample 8, 75 % iron, 10 % boron and 15 % neodymium by atoms: 31.9 MGOe.
Source: M. Sagawa et al. (Sumitomo Special Metals), US 4,770,723 (1988). Unknown: how the pure iron, the ferroboron and the neodymium metal are made; the patent does not say. The magnetising is ours, after Przybylski et al., Sensors 16:569 (2016). The 1 kg weights are our arithmetic from the patent's atomic percentages. Picture: the patent's Fig. 8.
خبير
2 days
التعليمات
1
1
Weigh sample 8: 75 Fe, 10 B, 15 Nd
Weigh sample 8: 75 Fe, 10 B, 15 Nd
Sample 8 is 75 % iron, 10 % boron and 15 % neodymium by atoms. Use 99.9 % electrolytic iron, ferroboron (19.38 % B, 5.32 % Al, 0.74 % Si, 0.03 % C, the rest iron) and neodymium of 99.7 % or better. Ours: a 1 kg melt, by arithmetic: 584.0 g iron, 86.4 g ferroboron, 334.9 g neodymium. Unknown: how these three are made.
المواد لهذه الخطوة:
حديد إلكتروليتي584 غ
فيروبورون86.4 غ
معدن النيوديميوم334.9 غالأدوات المطلوبة:
ميزان ذو كفّتين2
2
Melt by high frequency in argon and cast
Melt by high frequency in argon and cast
Melt the charge in a high-frequency (induction) furnace under argon and pour it into a water-cooled copper mould.
الأدوات المطلوبة:
فرن حثّي
بوتقة من طين حراري
أرغون
أسطوانة غاز مضغوط
قالب نحاسي مبرّد بالماء
قفّازات مقاومة للحرارة3
3
Stamp to 35 mesh, ball-mill to 3-10 µm
Stamp to 35 mesh, ball-mill to 3-10 µm
Crush the casting in a stamp mill until it passes a 35-mesh sieve. Then grind it in a ball mill for 3 hours, to 3-10 µm.
الأدوات المطلوبة:
مطحنة الدقّ
طقم مناخل (فتحات متدرّجة)
مطحنة كرات حديدية
نظارات أمان4
4
Press in a 10 kOe field at 1.5 t/cm²
Press in a 10 kOe field at 1.5 t/cm²
Line the powder up in a magnetic field of 10 kOe and press it at 1.5 tonnes per cm². Unknown: the size and shape of the magnets.
الأدوات المطلوبة:
مكبس بمجال مغناطيسي5
5
Sinter in argon at 1000-1200 °C
Sinter in argon at 1000-1200 °C
Sinter the compacts at 1000-1200 °C for about one hour in argon, then let them cool. Sample 8 measured 11.9 kG remanence, 8.0 kOe coercivity and 31.9 MGOe.
الأدوات المطلوبة:
فرن أنبوبي
أرغون
أسطوانة غاز مضغوط
قفّازات مقاومة للحرارة6
6
Magnetise the magnets
Magnetise the magnets
Ours, after Przybylski et al., Sensors 16:569 (2016): put each magnet in the coil of an impulse magnetiser and discharge a capacitor bank through it. They found a field of 1200 kA/m enough to saturate N38 sintered Nd-Fe-B; their magnetiser used a 1 mF bank charged up to 5000 V, a thyristor switch and a 440-turn coil of 3 mm copper wire with an 80 mm bore.
الأدوات المطلوبة:
جهاز المغنطةالمواد
3- 584 غعنصر نائب
- 86.4 غعنصر نائب
- 334.9 غعنصر نائب
الأدوات المطلوبة
14- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
- عنصر نائب
المخططات ذات الصلة
هذه المخططات تشارك المعرفة مع هذا — التقنيات والمواد والمبادئ
CC0 ملكية عامة
هذا المخطط مُصدر بموجب CC0. يحق لك نسخه وتعديله وتوزيعه واستخدامه لأي غرض، دون طلب إذن.
ادعم الصانع بشراء منتجات عبر مخططه حيث يكسب عمولة الصانع يحددها البائعون، أو أنشئ نسخة جديدة من هذا المخطط وضمّنه كرابط في مخططك لمشاركة الإيرادات.