Aqueous PTFE Dispersion: Tetrafluoroethylene Polymerised in Soapy Water (Berry 1951)
Ordinary soaps stop tetrafluoroethylene from growing into long chains. A fluorine soap does not: with 2 % of ammonium dodecafluoroheptanoate in the water, the gas polymerises into tiny PTFE ribbons that stay suspended. The result is a milky dispersion, a third of it polymer, the raw material for PTFE fine powder.
Source: K. L. Berry (du Pont), US 2,559,752 (1951), Example III. Making the ammonium salt from our acid, and the apparatus, are ours. Picture drawn by Youblob.
İleri
1 day
Talimatlar
1
1
Make the ammonium salt
Make the ammonium salt
Ours: neutralise about 1.9 parts of dodecafluoroheptanoic acid with ammonia solution until just neutral to litmus, giving 2 parts of ammonium dodecafluoroheptanoate. Make it up with distilled water to 93 parts of water in all. Parts are by weight.
Bu adım için malzemeler:
Dodekafloroheptanoik asit1.9 parts
Amonyak çözeltisi - %25-281 as required to neutralise
Damıtılmış Su93 partsGerekli aletler:
Turnusol kâğıdı
Cam kap
Eşit kollu terazi2
2
Load the pressure vessel
Load the pressure vessel
Put the solution in a pressure vessel with 0.05 part of potassium persulfate and 5 parts of paraffin wax melting at 56–58 °C. The wax protects the colloid while it is stirred.
Gerekli aletler:
Persülfat başlatıcı
Parafin
Basınçlı reaktör
Eşit kollu terazi3
3
Heat and remove the air
Heat and remove the air
Bring it to 80–85 °C, then evacuate the vessel and hold it under reduced pressure for several minutes to drive out air and dissolved oxygen.
Gerekli aletler:
Basınçlı reaktör
Vakum pompası
Termometre4
4
Feed tetrafluoroethylene for 3.6 hours
Feed tetrafluoroethylene for 3.6 hours
Let in tetrafluoroethylene to 60 lb/sq in gauge. Agitate at 80–85 °C for 3.6 hours; each time the pressure falls to 55 lb/sq in, bring it back to 60.
Bu adım için malzemeler:
Tetrafloroetilen1 as required to hold 55–60 psiGerekli aletler:
Basınçlı reaktör
Basınçlı gaz tüpü
Basınç Göstergesi
Termometre5
5
Cool and lift off the wax
Cool and lift off the wax
Cool it. The paraffin sets on top and lifts off. Below it is a colloidal PTFE dispersion with 34 % solids.
Gerekli aletler:
Basınçlı reaktör
Kapaklı Cam KavanozlarMalzemeler
4- 1.9 partsYer Tutucu
- 1 as required to neutraliseYer Tutucu
- 93 partsYer Tutucu
- 1 as required to hold 55–60 psiYer Tutucu
Gerekli Aletler
11- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- 1 vendor sell this, none ship to you yetYer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
Bu planla yapılan
İlgili Blueprint'ler
Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler

Tehlikeli
Dodecafluoroheptanoic Acid: the Fluoro Alcohol Oxidised with Permanganate (Berry 1951)
Charlie tarafından
Endüstriyel
2
0
0
0
0
0

Tehlikeli
Tetrafluoroethylene: Chlorodifluoromethane Pyrolysed in a Silver Tube at 700 °C
Charlie tarafından
Endüstriyel
9
0
0
0
0
0

PTFE Resin Powder: Tetrafluoroethylene Polymerised under Pressure, Plunkett 1941
Charlie tarafından
Endüstriyel
4
0
0
0
0
0
CC0 Kamu Malı
Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.
Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.