Barium Ferrite Disc Magnet: Barium Carbonate and Iron Oxide Sintered (Went, Philips 1956)
Charlie

Oluşturan

Charlie

28. Ekim 2026DE
1
0
0
0
0

Barium Ferrite Disc Magnet: Barium Carbonate and Iron Oxide Sintered (Went, Philips 1956)

The dark grey ceramic magnet on fridges and in loudspeakers is barium ferrite. It is made from two cheap powders: one part barium carbonate to six of iron oxide, milled, fired, milled again, pressed and sintered. No cobalt or nickel is needed. This is Example 34 of the Philips patent. Fired 4 hours at 1100 °C, its rod held 1,375 gauss with a coercive force of 3,350 oersted. Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956). They pressed rods; the claim covers "a body of a desired shape", and the disc size is ours. The patent does not say how to magnetise it; our way is stated. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
İleri
2 days

Talimatlar

1

Weigh one part barium carbonate to six of iron oxide

Weigh 39.5 g of barium carbonate (0.2 mol) and 191.7 g of ferric oxide, Fe2O3 (1.2 mol). Barium carbonate is poisonous if swallowed: ours, gloves and a dust respirator.

Bu adım için malzemeler:

Baryum karbonat (viterit)Baryum karbonat (viterit)39.5 g
Ferrik oksitFerrik oksit191.7 g

Gerekli aletler:

Eşit kollu teraziEşit kollu terazi
Lastik eldivenLastik eldiven
P100 Solunum MaskesiP100 Solunum Maskesi
2

Mill with ethanol for 4 hours

Grind the mixture with ethanol in an iron ball mill for 4 hours. Let the ethanol evaporate, then dry the powder in a drying oven.

Gerekli aletler:

Demir Bilyalı DeğirmenDemir Bilyalı Değirmen
Etanol - laboratuvar kalitesi, %95Etanol - laboratuvar kalitesi, %95
Kurutma fırınıKurutma fırını
3

Presinter at 1000 °C for 4 hours

Fire the dry powder in air at 1000 °C for 4 hours (ours: in a lidded porcelain crucible in a muffle furnace). Let it cool.

Gerekli aletler:

Mufla fırınMufla fırın
Kapaklı kroze (porselen)Kapaklı kroze (porselen)
Pota MaşasıPota Maşası
Isıya Dayanıklı EldivenIsıya Dayanıklı Eldiven
4

Mill again for 4 hours

Grind the presintered product with ethanol in the ball mill for another 4 hours. Let the ethanol evaporate.

Gerekli aletler:

Demir Bilyalı DeğirmenDemir Bilyalı Değirmen
Etanol - laboratuvar kalitesi, %95Etanol - laboratuvar kalitesi, %95
Kurutma fırınıKurutma fırını
P100 Solunum MaskesiP100 Solunum Maskesi
5

Press discs at 1.5 tons per cm²

Press the powder at 1.5 tons/cm². The patent pressed rods; we press discs. Ours: a die 20 mm across, so about 4.7 tonnes on the punch (our arithmetic: 1.5 × 3.14 cm²).

Gerekli aletler:

Hidrolik presHidrolik pres
Disk presleme kalıbıDisk presleme kalıbı
6

Sinter for 4 hours

Sinter the discs for 4 hours in oxygen or in air. The patent's results: at 1100 °C, 1,375 gauss and 3,350 oersted; at 1200 °C, 1,400 and 3,100; at 1300 °C, 1,850 and 1,780. Hotter gives a stronger but less stubborn magnet.

Gerekli aletler:

Mufla fırınMufla fırın
Pota MaşasıPota Maşası
Isıya Dayanıklı EldivenIsıya Dayanıklı Eldiven
7

Magnetise the discs

The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.

Gerekli aletler:

ElektromıknatısElektromıknatıs
PusulaPusula

Malzemeler

2

Gerekli Aletler

14

CC0 Kamu Malı

Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.

Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.

Tartışma

(0)

Giriş yapın tartışmaya katılmak için

Yorumlar yükleniyor...