Bismuth: Sweated Out of Native Ore in Inclined Iron Tubes, the Schneeberg Way (Thorpe, 1912)
Charlie

Oluşturan

Charlie

4. Kasım 2026DE
13
0
0
0
0

Bismuth: Sweated Out of Native Ore in Inclined Iron Tubes, the Schneeberg Way (Thorpe, 1912)

The old way of getting bismuth from ore that holds it as the metal: heat the lumps just enough in sloping iron tubes and the bismuth, which melts easily, runs out of the rock into pots under charcoal. It takes 30-60 minutes a charge but gets only about two-thirds of the metal. Not given: the furnace temperature. Source: E. Thorpe, Dictionary of Applied Chemistry vol. I (1912), Bismuth, p. 458. Picture: Thorpe's Fig. 1, the furnace in plan.
Orta
30-60 minutes per charge

Talimatlar

1

Pick and break the ore

Sort the ore (7-12 % bismuth) by hand from the waste rock as far as possible and break it into pieces the size of a hazel nut.

Bu adım için malzemeler:

Doğal bizmut cevheriDoğal bizmut cevheri1 12 cwt per tube charge

Gerekli aletler:

ÇekiçÇekiç
Endüstriyel platform kantarıEndüstriyel platform kantarı
2

Charge the tubes

Load about 12 cwt into each inclined iron tube of the furnace, leaving room to stir from the upper end. Close the upper ends with iron plates and the lower ends with plates pierced with round holes. Under each lower end stand an iron pot holding powdered charcoal, kept gently warm by a small charcoal fire.

Bu adım için malzemeler:

Odun KömürüOdun Kömürü1 powdered, in the pots and for the pot fire

Gerekli aletler:

Bizmut sıvılaştırma fırınıBizmut sıvılaştırma fırını
Demir potaDemir pota
3

Sweat out the bismuth

Fire the furnace with wood so that the metal flows easily. In about 10 minutes the bismuth begins to run into the pots, where the charcoal covers it from the air. Stir the ore now and then with an iron rod from the upper end; in 30-60 minutes the charge is done. 20 cwt of ore burns about 63 cubic feet of wood.

Bu adım için malzemeler:

Yakacak OdunYakacak Odun1 about 63 cu ft per 20 cwt of ore

Gerekli aletler:

Bizmut sıvılaştırma fırınıBizmut sıvılaştırma fırını
Yuvarlak demir çubukYuvarlak demir çubuk
4

Rake out and recharge

Rake the spent ore (bismuth barley) out of the upper end into the tank and refill at once with fresh ore.

Gerekli aletler:

Demir tırmıkDemir tırmık
Bizmut sıvılaştırma fırınıBizmut sıvılaştırma fırını
5

Cast ingots

Ladle the bismuth from the pots into moulds and cast ingots of 25-50 lb.

Gerekli aletler:

Demir potaDemir pota
Döküm kepçesiDöküm kepçesi
Külçe kalıbıKülçe kalıbı

Malzemeler

3
  • 1 12 cwt per tube charge
    Yer Tutucu
  • 1 powdered, in the pots and for the pot fire
    Yer Tutucu
  • 1 about 63 cu ft per 20 cwt of ore
    Yer Tutucu

Gerekli Aletler

8

Bu planla yapılan

CC0 Kamu Malı

Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.

Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.

Tartışma

(0)

Giriş yapın tartışmaya katılmak için

Yorumlar yükleniyor...