Bouncing Putty
Looking for a synthetic rubber during the Second World War, James Wright at General Electric heated silicone oil with boric acid. The result was no rubber: it bounced, shattered under a hammer, stretched like toffee when pulled slowly and slumped into a puddle overnight. Nobody found an industrial use; in 1950 it was sold as a toy.
**US 2,541,851**, "Process for making puttylike elastic plastic, siloxane derivative composition containing zinc hydroxide", Wright, assigned to General Electric, filed 23. December 1944, granted 13. February 1951: liquid dimethylsiloxane heated with 5 to 25 % by weight of a boron compound such as boric acid or borax.
**You measure both of its lives**: how high it bounces, how fast it flows, and where one turns into the other.
Başlangıç
1 hour plus a day of slumping
Talimatlar
1
1
Weigh a ball
Weigh a ball
Weigh out 20 g of bouncing putty and roll it into a smooth ball between your palms.
Bu adım için malzemeler:
Zıplayan macun20 gGerekli aletler:
Hassas Dijital Terazi2
2
Bounce it
Bounce it
Tape a tape measure up a wall. Drop the ball from 1.0 m onto a hard floor five times, filming in slow motion, and read each rebound height.
Bu adım için malzemeler:
Maskeleme bandı1 ruloGerekli aletler:
Şerit Metre
Ağır Çekim Video Çeken Akıllı Telefon3
3
Pull slow, pull fast
Pull slow, pull fast
Roll a 10 mm thick rope. Pull one over 10 seconds: it strings out. Pull another sharply: it snaps with a clean face. Try pull times in between and note the fastest pull that still stretches.
Gerekli aletler:
Kronometre
Metal cetvel4
4
Strike it
Strike it
Glasses on. Set a ball on a hard surface and hit it once, sharply, with the mallet. It cracks rather than squashing. Squash another slowly with your thumb.
Gerekli aletler:
Kauçuk tokmak
Şeffaf Koruyucu Gözlük5
5
Let it slump
Let it slump
Re-roll the 20 g ball and set it on wax paper on a level surface. Measure its diameter now and after 10, 30, 60 and 180 minutes and 24 hours.
Bu adım için malzemeler:
Mumlu kağıt1 yaprakGerekli aletler:
Dijital Kumpas 6 İnç6
6
Deborah numbers
Deborah numbers
Jupyter defteri yükleniyor…
7
7
History & Context
History & Context
**What the patent specifies:** liquid dimethylsiloxane heated with 5–25 % of a boron compound until putty-like. **Modern build (derived):** commercial bouncing putty, measured.
It became a famous toy and a staple of physics teaching about materials that are neither simply solid nor simply liquid. Its limits: it picks up dirt, will not hold a shape, and flows out of any container that is not closed.
Malzemeler
3- 20 gYer Tutucu
- 1 ruloYer Tutucu
- 1 yaprakYer Tutucu
Gerekli Aletler
8- Yer Tutucu
- 1 vendor sell this, none ship to you yetYer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
İlgili Blueprint'ler
Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler
CC0 Kamu Malı
Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.
Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.