Carbon Resistance Ring: Laminated Paper Gelled with 15% Tung Oil, Graphite-Shellac Track
Mallory's quiet volume-control ring (US 2,144,925, 1939). Hard bases were noisy and soft paper ones changed with damp. Their answer: paper rings soaked in 15 % raw tung oil and baked, so the oil gels inside the paper. It shuts out moisture but stays soft and springy, and the wiper runs on it quietly. A graphite paint makes the track, silver paint the ends.
The picture: the patent's drawing (Fig. 3).
Orta
1 day
Talimatlar
1
1
Punch rings from three-ply paper
Punch rings from three-ply paper
The base is three papers stuck into one sheet: litho paper at the back, newsprint in the middle, manila on the face that takes the track. Punch rings from it. Ours: a punch press with a ring die.
Bu adım için malzemeler:
Üç katlı laminasyonlu kâğıt1 adetGerekli aletler:
Zımba presi
Halka delme kalıbı
Lastik eldiven2
2
Soak 1 hour in 15 % tung oil in naphtha
Soak 1 hour in 15 % tung oil in naphtha
Soak the rings for about one hour in about 15 % raw tung oil in naphtha. Use raw oil, not heat-bodied or treated oil, so it can still gel.
Bu adım için malzemeler:
Tung yağı15 partsGerekli aletler:
Nafta
Cam Beher
Eşit kollu terazi
Karıştırıcı
Tam yüz maskesi
Lastik eldiven3
3
Air-dry, then bake at 210–250 °C
Air-dry, then bake at 210–250 °C
Dry the rings in air for two hours or more, then bake 15 to 30 minutes at 210 to 250 °C. The oil gels in the paper's pores; the paper stays pliable.
Gerekli aletler:
Kurutma fırını
Fırın Termometresi
Isıya Dayanıklı Eldiven4
4
Spray the graphite track
Spray the graphite track
Spray on the resistance paint, for example graphite in a shellac binder. The patent gives no proportions. The track can be tapered in thickness, width or mix to shape the resistance curve.
Bu adım için malzemeler:
Grafit Tozu1 as required
Gomalak1 as requiredGerekli aletler:
Sprey Tabancası
Hava kompresörü
Tam yüz maskesi
Lastik eldiven5
5
Paint silver ends, bake at 220 °C
Paint silver ends, bake at 220 °C
Spray or paint the two end terminals with silver particles in shellac. Dry, then bake at about 220 °C to cure and harden the track. The slight warp from soaking flattens out again.
Bu adım için malzemeler:
Gümüş iletken boya1 as requiredGerekli aletler:
Sprey Tabancası
Kurutma fırını
Fırın Termometresi
Isıya Dayanıklı EldivenMalzemeler
5- Yer Tutucu
- 15 partsYer Tutucu
- 1 as requiredYer Tutucu
- 1 as requiredYer Tutucu
- 1 as requiredYer Tutucu
Gerekli Aletler
13- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- 1 vendor sell this, none ship to you yetYer Tutucu
Bu planla yapılan
İlgili Blueprint'ler
Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler
CC0 Kamu Malı
Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.
Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.