Ceramic Disc Capacitors: Barium Titanate with Nickel Stannate, Pressed, Fired and Silvered (Coffeen, US 2,789,061)
Ed

Oluşturan

Ed

2. Kasım 2026FI
1
0
0
0
0

Ceramic Disc Capacitors: Barium Titanate with Nickel Stannate, Pressed, Fired and Silvered (Coffeen, US 2,789,061)

Barium titanate with 3 mole % nickel stannate is calcined, pressed into small discs and fired hard. Silver is fired onto both faces and a lead soldered to each, giving ceramic disc capacitors of high capacity for their size. Result: discs 3/8 inch across and about 1/10 inch thick with a dielectric constant averaging 2380 and a dissipation factor of 0.58 %. Between 25 and 85 °C the dielectric constant rose at most 17 % and fell at most 7 %. Source: W. W. Coffeen (Metal & Thermit Corp.), US 2,789,061 (1957). Unknown: how the barium titanate, the nickel stannate and the tinned lead wire are made; the patent uses them ready-made. Picture: Wikimedia Commons.
İleri
10 days

Talimatlar

1

Weigh and slurry

Weigh 19.32 g of barium titanate and 0.68 g of hydrated nickel stannate (about NiSnO3·2H2O), which is 97 mole % BaTiO3 and 3 mole % NiSnO3. Slurry them with 50 cc of distilled water. The patent prefers 2 to 4 mole % nickel stannate; 1 to 15 % works.

Bu adım için malzemeler:

Baryum titanatBaryum titanat19.32 g
Nikel stannatNikel stannat0.68 g

Gerekli aletler:

Damıtılmış SuDamıtılmış Su
Hassas Dijital TeraziHassas Dijital Terazi
Buharlaştırma KabıBuharlaştırma Kabı
2

Dry, sieve and calcine

Dry the slurry, crush it to pass a 50 mesh screen, moisten it with 5 % of a 2 1/2 % starch solution and press it into one slug. Calcine the slug for one hour at 1600 °F (871 °C). Ours: potato starch, a drying oven, mortar and pestle.

Gerekli aletler:

Patates nişastasıPatates nişastası
Kurutma fırınıKurutma fırını
Havan ve HavaneliHavan ve Havaneli
KalburKalbur
Hidrolik presHidrolik pres
Yüksek sıcaklık fırınıYüksek sıcaklık fırını
3

Press the discs

Grind the calcine to pass a 325 mesh screen, moisten it again with starch solution, and press small discs 3/8 inch in diameter and about 1/10 inch thick at 20,000 pounds per square inch.

Gerekli aletler:

Havan ve HavaneliHavan ve Havaneli
İnce Gözlü Elekİnce Gözlü Elek
Patates nişastasıPatates nişastası
Hidrolik presHidrolik pres
Disk presleme kalıbıDisk presleme kalıbı
4

Fire on platinum

Fire the discs on platinum foil at 2400 °F (1316 °C) for one hour. They come out with zero absorption.

Gerekli aletler:

Yüksek sıcaklık fırınıYüksek sıcaklık fırını
PlatinPlatin
5

Silver and lead

Paint silver paint on both faces and fire the discs at 1350 °F (732 °C) for one hour. Solder tinned copper lead wires directly to the silver electrodes. Age at least a week before measuring. Ours: a fine brush and a soldering iron.

Bu adım için malzemeler:

Pişirmeli gümüş boyaPişirmeli gümüş boya1 both faces
Kalaylı bakır telKalaylı bakır tel2 leads per disc
Lehim TeliLehim Teli1 a little

Gerekli aletler:

İnce uçlu fırçalarİnce uçlu fırçalar
Yüksek sıcaklık fırınıYüksek sıcaklık fırını
HavyaHavya

Malzemeler

5

Gerekli Aletler

14

CC0 Kamu Malı

Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.

Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.

Tartışma

(0)

Giriş yapın tartışmaya katılmak için

Yorumlar yükleniyor...