Chromium Metal: Chromic Oxide Reduced by Aluminium (Thermit)
Forge

Oluşturan

Forge

18. Ekim 2026NO
17
0
0
0
0

Chromium Metal: Chromic Oxide Reduced by Aluminium (Thermit)

Aluminium takes the oxygen from chromic oxide with so much heat that the chromium comes out molten. Thorpe (1912-13) gives Goldschmidt's thermit: chromic oxide mixed with aluminium powder in a magnesia-lined crucible, lit through a fuse of aluminium powder and barium peroxide with a magnesium ribbon. The heat carries the reaction through the whole charge, and carbon-free chromium sinks under a slag of alumina. White heat: outdoors on dry sand, face shield, stand well back. The picture: chromium metal (Wikimedia Commons).
İleri
1 day

Talimatlar

1

Line the crucible

Line a refractory crucible with a paste of magnesia and water glass, and let it dry fully.

Gerekli aletler:

Ateş Kili PotasıAteş Kili Potası
Magnezyum oksitMagnezyum oksit
Su camı (sodyum silikat çözeltisi)Su camı (sodyum silikat çözeltisi)
2

Mix the charge

Weigh 150 g of dry chromic oxide and 50 g of aluminium powder, a little less than the 53 g the equation needs, and mix them intimately.

Bu adım için malzemeler:

Krom OksitKrom Oksit150 g
Alüminyum TozuAlüminyum Tozu50 g

Gerekli aletler:

Eşit kollu teraziEşit kollu terazi
Havan ve HavaneliHavan ve Havaneli
3

Set the fuse

Stand the crucible on dry sand outdoors and fill in the charge. On top put a small heap of aluminium powder mixed with barium peroxide, and push a strip of magnesium ribbon into it.

Bu adım için malzemeler:

Alüminyum TozuAlüminyum Tozu1 adet
Baryum peroksitBaryum peroksit1 adet
Magnezyum ŞeritMagnezyum Şerit1 adet

Gerekli aletler:

Kuru kum kovasıKuru kum kovası
4

Light it and stand back

Face shield on. Light the end of the ribbon and step well back. The fuse fires the charge and the reaction runs through it by its own heat.

Gerekli aletler:

ÇakmakÇakmak
Yüz SiperliğiYüz Siperliği
Deri EldivenDeri Eldiven
5

Break out the regulus

Let it cool completely. Break away the alumina slag on top and take out the button of chromium from the bottom. At most 103 g can form from 150 g of oxide.

Gerekli aletler:

ÇekiçÇekiç
Deri EldivenDeri Eldiven
Yüz SiperliğiYüz Siperliği
Kapaklı Cam KavanozlarKapaklı Cam Kavanozlar

Malzemeler

4

Gerekli Aletler

11

CC0 Kamu Malı

Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.

Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.

Tartışma

(0)

Giriş yapın tartışmaya katılmak için

Yorumlar yükleniyor...