Iron plated out of a fresh green ferrous bath comes off rough and useless. Bouchayer first stirred the bath in air until it turned bright brown; the iron oxychloride formed takes care of the hydrogen at the cathode, and the deposit grows even and compact at high current. Result: electrolytic iron, deposited at about 98 % current yield. Source: Bouchayer, US 1,516,326 (1924). Not given: cathode material, purity of the iron. Picture drawn by Youblob.
İleri
Factory process

Talimatlar

1

Make up the electrolyte at 20 °Bé

Dissolve ferrous sulfate in water (Bouchayer also allows ferrous chloride or a mix). Concentration: e.g. 20 °Bé, then keep it constant.

Bu adım için malzemeler:

Demir sülfatDemir sülfat1 as required

Gerekli aletler:

SuSu
HidrometreHidrometre
Elektroliz tankıElektroliz tankı
2

Stir it in air until brown

Agitate the green bath in air, e.g. by turning the anode, until it is bright brown and stops foaming. Used green, it gives only an irregular deposit.

Gerekli aletler:

Elektroliz tankıElektroliz tankı
3

Circulate it through iron filings

Pump the electrolyte through a mass of iron filings in a separate vessel; it takes back iron and forms the ferric hydroxide that keeps the bath working. Keep it moving fast past the anodes: this lowers the phosphorus.

Bu adım için malzemeler:

Demir talaşıDemir talaşı1 as required

Gerekli aletler:

Su pompasıSu pompası
4

Deposit on a rotating cathode

Electrolyse between graphite anodes and a rotating cathode. Temperature: e.g. 75-77 °C at 1000 A/m², held exactly constant and below boiling; cathode speed: e.g. 120 m/min at 800 A/m². Cathode material: not given.

Gerekli aletler:

Grafit elektrotGrafit elektrot
Doğru akım güç kaynağıDoğru akım güç kaynağı
TermometreTermometre
Elektroliz tankıElektroliz tankı
5

Strip and reheat the deposit

Take the compact iron deposit off the cathode; it is usable after a slight reheating (temperature not given).

Gerekli aletler:

Elektroliz tankıElektroliz tankı

Malzemeler

2

Gerekli Aletler

7

CC0 Kamu Malı

Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.