Equilateral Glass Prism: Sawn, Ground and Pitch-Polished

A prism splits white light into its colours, so its faces must be optically flat and its angles true. This is how the US arsenals ground prisms in 1918, as F. E. Wright recorded for the Ordnance Department in 1921: saw a blank from optical glass, rough-grind it on iron disks, set a batch of prisms in plaster, fine-grind, and polish on pitch with rouge. Wright's worked example is a right-angle prism; an equilateral prism has three 60° angles, made the same way. The picture: blocking prisms for rough grinding at Frankford Arsenal (Wright 1921, Fig. 77, public domain).
İleri
2-3 days

Talimatlar

1

Saw out the blank

Saw a triangular blank from a block of optical glass with a diamond saw, using kerosene as lubricant. Leave several millimetres extra on each face for grinding.

Bu adım için malzemeler:

Optik CamOptik Cam1 as required

Gerekli aletler:

Elmas TestereElmas Testere
GazyağıGazyağı
Dijital Kumpas 6 İnçDijital Kumpas 6 İnç
Koruyucu gözlükKoruyucu gözlük
2

Rough-grind the faces

Grind one triangular end flat on a rotating iron disk with 90 or 150 mesh grit. Then rough out the three side faces at right angles to it, checking the 60° angles with an angle gauge.

Gerekli aletler:

Demir Taşlama DiskiDemir Taşlama Diski
Silisyum karbür aşındırıcı tane setiSilisyum karbür aşındırıcı tane seti
Açı MastarıAçı Mastarı
3

Grind the ends in a batch

Wax 20 or more prisms by their ground ends onto a heated iron disk and grind the other ends together: 90, 150, then 220 mesh, then smoothing grit. Change grit only when the surface is free of scratches. Regrind to the set thickness.

Gerekli aletler:

Demir Taşlama DiskiDemir Taşlama Diski
Silisyum karbür aşındırıcı tane setiSilisyum karbür aşındırıcı tane seti
ParafinParafin
BalmumuBalmumu
Isıtıcı TablaIsıtıcı Tabla
Dijital Kumpas 6 İnçDijital Kumpas 6 İnç
4

Block the prisms in plaster

Set the prisms face down in melted paraffin on a flat iron disk and coat their backs with beeswax. Clamp a ring round them, fill with plaster of Paris and a little Portland cement (10 : 1), and let it harden about 16 hours. Cut the plaster back 1/8 in from the prisms and give it two coats of shellac.

Gerekli aletler:

Isıtıcı TablaIsıtıcı Tabla
ParafinParafin
BalmumuBalmumu
Alçı (Paris Alçısı)Alçı (Paris Alçısı)
Portland çimentosuPortland çimentosu
Bal Mumu PeletiBal Mumu Peleti
5

Fine-grind

Grind the block on a slightly convex plate with wet flour emery (the part that settles out of water between 10 and 60 minutes). After five minutes check with a magnifier: the faces should have an even velvet finish, slightly hollow by less than 0.001 in.

Gerekli aletler:

Demir Taşlama DiskiDemir Taşlama Diski
Silisyum karbür aşındırıcı tane setiSilisyum karbür aşındırıcı tane seti
Büyüteç LupuBüyüteç Lupu
6

Polish on pitch

Pour strained pitch with a little rosin 1/4 in deep on an iron tool and cut crossed grooves 1/8 in wide, 1 in apart. Press it true with a rouge-wetted flat. Polish the block with creamy rouge and water on the machine, usually 4–8 hours, running nearly dry at the end.

Gerekli aletler:

Odun katranı ziftiOdun katranı zifti
Çam reçinesi (kolofan)Çam reçinesi (kolofan)
Kuyumcu kırmızısıKuyumcu kırmızısı
Optik Parlatma MakinesiOptik Parlatma Makinesi
7

Test for flatness

Lay an optical flat on each face and look at the Newton colours in sodium light (salt in a Bunsen flame). Straight bands to the edge, or one colour over the whole face, mean it is flat.

Gerekli aletler:

Optik düzlem (referans)Optik düzlem (referans)
Bunsen bekiBunsen beki
TuzTuz
Büyüteç LupuBüyüteç Lupu
8

Free, clean, check the angle, repeat

Break the plaster away, clean the prisms with benzene and check each angle with the angle gauge. Correct by hand on a flat tool with smoothing grit. Repeat blocking and polishing for every face, smallest face first.

Gerekli aletler:

ÇekiçÇekiç
BenzenBenzen
Açı MastarıAçı Mastarı
Demir Taşlama DiskiDemir Taşlama Diski
Silisyum karbür aşındırıcı tane setiSilisyum karbür aşındırıcı tane seti

Malzemeler

1
  • 1 as required
    Yer Tutucu

Gerekli Aletler

23

İlgili Blueprint'ler

Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler

CC0 Kamu Malı

Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.

Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.

Tartışma

(0)

Giriş yapın tartışmaya katılmak için

Yorumlar yükleniyor...