Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 50 °C (McIntire, Dow 1948, Ex. 3, Test 2)
Charlie

Oluşturan

Charlie

28. Ekim 2026DE
1
0
0
0
0

Extruded Polystyrene Foam: Propylene-Blown Log Let Out at 50 °C (McIntire, Dow 1948, Ex. 3, Test 2)

Extruded polystyrene foam blown with a propylene gas fraction instead of methyl chloride. Polystyrene stands two days at 40 °C with the propylene under pressure and becomes a gel. Let out at 50 °C (250 psi in the tower), it swelled into a log 6 to 9 inches across, weighing 4.8 lb per cubic foot, with somewhat smaller, uniform cells. Source: O. R. McIntire (Dow), US 2,450,436 (1948), Example 3. Picture: the patent's drawing.
İleri
3 days

Talimatlar

1

Charge the tower with polystyrene

Charge a high-pressure tower with 300 lb of granular polystyrene.

Bu adım için malzemeler:

PolistirenPolistiren300 libre

Gerekli aletler:

Basınçlı reaktörBasınçlı reaktör
Eşit kollu teraziEşit kollu terazi
Lastik eldivenLastik eldiven
2

Add the propylene fraction

Add 100 lb of a cracked-oil gas fraction that is about 93 % propylene, under pressure, and close the tower. Propylene is a flammable gas: no flames, strong ventilation.

Bu adım için malzemeler:

PropilenPropilen100 libre

Gerekli aletler:

Basınçlı gaz tüpüBasınçlı gaz tüpü
Basınçlı reaktörBasınçlı reaktör
Kimyasal Sıçrama GözlüğüKimyasal Sıçrama Gözlüğü
3

Stand two days at 40 °C

Let the tower stand for two days at 40 °C while the polystyrene takes up the propylene.

Gerekli aletler:

Basınçlı reaktörBasınçlı reaktör
Laboratuvar TermometresiLaboratuvar Termometresi
4

Let it out at 50 °C

Open the valved outlet near the bottom (3.25 inch in the patent) at 50 °C. The pressure is about 250 psi. The gel flows out and swells into a log 6 to 9 inches across, 4.8 lb per cubic foot, with somewhat smaller, uniform cells. Close the outlet again. The patent heated step by step (50, 60, 75 °C) for several hours each, letting a portion out at each step.

Gerekli aletler:

Basınçlı reaktörBasınçlı reaktör
Laboratuvar TermometresiLaboratuvar Termometresi
Kimyasal Sıçrama GözlüğüKimyasal Sıçrama Gözlüğü
Lastik eldivenLastik eldiven
5

Saw into boards

When the foam has set, saw it lengthwise into slabs (ours: a woodworking saw).

Gerekli aletler:

Marangoz testeresiMarangoz testeresi
Lastik eldivenLastik eldiven

Malzemeler

2
  • 300 libre
    Yer Tutucu
  • 100 libre
    Yer Tutucu

Gerekli Aletler

7

CC0 Kamu Malı

Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.

Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.