Ferrite Toroid Core: Copper-Zinc Ferrite Sintered at 1100 °C (Snoek 1948, Ex. I)
Charlie

Oluşturan

Charlie

28. Ekim 2026DE
0
0
0
0
0

Ferrite Toroid Core: Copper-Zinc Ferrite Sintered at 1100 °C (Snoek 1948, Ex. I)

A soft ferrite ring core for coils and transformers: copper, zinc and iron oxides with a little brownstone, pressed into a ring and sintered at 1100 °C in oxygen. Snoek's ring had an initial permeability of 118. Source: J. L. Snoek, US 2,452,530 (Philips, 1948), Example I and its table. Unknown: the 'violet' iron oxide, linked to an unknown head. Picture: the patent's Fig. 4, the ring core.
İleri
2 days

Talimatlar

1

Weigh 20 : 30 : 50 mol % and 1 % brownstone

Mix 20 mol % pure copper oxide, 30 mol % pure zinc oxide and 50 mol % pure violet iron oxide, and add 1 % by weight of brownstone (manganese dioxide). Ours, by weight: 13.24 g copper oxide, 20.32 g zinc oxide and 66.44 g iron oxide per 100 g, plus 1 g brownstone. Unknown: what makes the iron oxide 'violet'; Snoek does not say.

Bu adım için malzemeler:

Bakır OksitBakır Oksit13.24 g
Çinko Oksit TozuÇinko Oksit Tozu20.32 g
Mor demir oksitMor demir oksit66.44 g
Manganez dioksit (pirolusit)Manganez dioksit (pirolusit)1 g

Gerekli aletler:

Eşit kollu teraziEşit kollu terazi
Toz MaskesiToz Maskesi
2

Grind half an hour in an iron ball mill

Grind the mixture for half an hour in a mill with iron balls.

Gerekli aletler:

Demir Bilyalı DeğirmenDemir Bilyalı Değirmen
Toz MaskesiToz Maskesi
3

Press a ring at 4 tons per cm²

Press the powder at 4 tons per square centimetre into a ring 3 cm across with a 4 × 4 mm cross-section.

Gerekli aletler:

Hidrolik presHidrolik pres
Halka Presleme KalıbıHalka Presleme Kalıbı
Toz MaskesiToz Maskesi
4

Sinter at 1100 °C in oxygen, cool 5–10 °C a minute

Sinter the ring at 1100 °C in a current of oxygen. Example I heats for 1 hour and cools in the oxygen at 5 to 10 °C per minute. Snoek's ring had an initial permeability of 118, measured at room temperature at 2 kHz.

Gerekli aletler:

Tüp FırınTüp Fırın
OksijenOksijen
Basınçlı gaz tüpüBasınçlı gaz tüpü
PirometrePirometre
Pota MaşasıPota Maşası
Isıya Dayanıklı EldivenIsıya Dayanıklı Eldiven

Malzemeler

4

Gerekli Aletler

11

CC0 Kamu Malı

Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.

Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.

Tartışma

(0)

Giriş yapın tartışmaya katılmak için

Yorumlar yükleniyor...