Glass Tube: Drawn by Two Glassmakers Walking Apart (Pellatt, 1849)
How glass tube was made by hand: a blown gather of glass is welded at one end to a second rod, and two workers walk away from each other while turning, stretching the hot glass into a tube up to 60 or 70 feet long. Because the whole bubble stretches evenly, the bore and the wall stay in the same proportion all along the tube.
Result: long glass tube of nearly even bore, cut into lengths when cold. Solid cane is made the same way without blowing.
Source: Apsley Pellatt, Curiosities of Glass Making (1849), pp. 106-108. Unknown: the glass batch and the gather's size. Picture: the book's figures.
Uzman
Unknown
Talimatlar
1
1
Gather and blow the ball
Gather and blow the ball
Gather a solid ball of flint glass on the end of the blowing iron and blow it out a little, so it is hollow. When it has partly cooled, use it as a core for one or more further gatherings until there is enough glass. For flat-bore thermometer tube, flatten the first ball on the marver with an iron or wooden battledore before the later gatherings. Ours: lead crystal. Not given: the amount of glass.
Bu adım için malzemeler:
Kurşunlu kristal1 flint glassGerekli aletler:
1100 santigrat dereceye çıkabilen cam fırını
Cam üfleme çubuğu
Marver (cam yuvarlama plakası)2
2
Swing it long and fix the post
Swing it long and fix the post
Lengthen the ball by swinging it, and chill its far end by dipping it in cold water. A second worker makes a disc of hot glass on a rod, the 'post', and holds it upright near the ground. The chief worker climbs onto a chair and drops the hot ball onto the post, where it welds on.
Gerekli aletler:
Su
Pontil çubuğu3
3
Walk apart and draw
Walk apart and draw
The chief worker steps down and the two walk away from each other, both turning their rods all the time. At first the hot glass sags between them in a curve; fan the parts that are thicker to cool them, so it stretches evenly. Draw it to the length wanted, up to 60 or 70 feet; as it cools it stops turning and pulls nearly straight. Except at the ends, it has nearly one bore, diameter and wall thickness. Ours: a wooden paddle for fanning (Pellatt: a boy's hat).
Gerekli aletler:
Cam üfleme çubuğu
Pontil çubuğu
Ahşap kürek4
4
Lay down and cut
Lay down and cut
Lay the tube across the wooden rungs of a ladder to cool. Cut it into lengths by touching it with a cold iron or nicking it with a steel file.
Gerekli aletler:
Ahşap merdiven
Metal EğeMalzemeler
1- 1 flint glassYer Tutucu
Gerekli Aletler
8- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
Bağlı Plan Malzemeleri
Bu planla yapılan
CC0 Kamu Malı
Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.
Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.