Lactide: Lactic Acid Condensed and Cracked under Vacuum, Recrystallised
Lactide is the ring-shaped double molecule of lactic acid, the monomer from which PLA is made. Schneider's du Pont patent (US 2,703,316, 1955) drives the water out of lactic acid, condenses it under vacuum to a syrupy low polymer, then heats that to 200–250 °C at 8–10 mm so that lactide distils off. For a tough plastic it must be very pure: recrystallise it from ethyl acetate until it melts at 120 °C or higher (best 123–125 °C).
The picture: our diagram.
İleri
1–2 days
Talimatlar
1
1
Drive off the water
Drive off the water
Distil the lactic acid at atmospheric pressure at 120–130 °C until nearly all the water of dilution has gone.
Bu adım için malzemeler:
Laktik Asit (teknik)1 adetGerekli aletler:
Yuvarlak dipli balon
Yoğuşturucu serpantini
Isıtıcı Tabla
Yağ Banyosu
Laboratuvar Termometresi2
2
Condense under vacuum
Condense under vacuum
Continue distilling under 17–35 mm of mercury. Water of esterification comes off and the acid becomes a syrupy low polymer (polylactic acid).
Gerekli aletler:
Vakum pompası
Vakum göstergesi
Soğuk Tuzak
Yağ Banyosu
Laboratuvar Termometresi3
3
Crack to lactide
Crack to lactide
Lower the pressure to 8–10 mm and raise the temperature to 200–250 °C. Lactide distils at 130–140 °C (10–13 mm) and sets to a soft crystalline solid.
Gerekli aletler:
Vakum pompası
Vakum göstergesi
Yoğuşturucu serpantini
Yağ Banyosu
Laboratuvar Termometresi
Isıya Dayanıklı Eldiven4
4
Recrystallise from ethyl acetate
Recrystallise from ethyl acetate
Recrystallise the crude lactide from ethyl acetate, filter and dry. Repeat: in the patent the melting point rose from 114–115 °C after the first crystallisation to 118, 123–124 and 124–125 °C after the fourth.
Gerekli aletler:
Etil Asetat
Isıya Dayanıklı Cam Beher
Isıtıcı Tabla
Büchner hunisi (porselen)
Süzgeç Kâğıdı
Kimyasal Sıçrama Gözlüğü5
5
Check the melting point
Check the melting point
Put a few crystals in a capillary tube and warm slowly. Lactide melting at 120 °C or above is fit for making PLA; below 120 °C it gives a brittle polymer.
Gerekli aletler:
Cam kılcal boru
Laboratuvar Termometresi
Yağ BanyosuMalzemeler
1- 1 adetYer Tutucu
Gerekli Aletler
15- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- 1 vendor sell this, none ship to you yetYer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
Bu planla yapılan
İlgili Blueprint'ler
Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler
CC0 Kamu Malı
Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.
Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.