Chamois Wash Leather: Frized Pelts Fulled With Fish Oil Eight or Nine Times (Morfit, 1852)
Oil-tawed chamois or wash leather, from Campbell Morfit's Arts of Tanning, Currying and Leather-Dressing (1852): sheep, goat or deer pelts with the grain rubbed off, beaten again and again with fish oil until it is worked right in, warmed so the oil sets in the fibre, then washed of excess oil in weak potash lye and finished soft. No tannin, no alum.
İleri
About 2 weeks
Talimatlar
1
1
Oil budget
Oil budget
Jupyter defteri yükleniyor…
2
2
Read The Arts of Tanning
Read The Arts of Tanning
"Oiled leather is commonly known as chamois, or wash-leather ... from its property of bearing wetting and washing."
3
3
Make pelts and friz
Make pelts and friz
Choose the finest goat, sheep, lamb or deer skins (or thin split sides). Bring them to pelt as for kid leather: wash, lime, fleece, beam and bran. Then friz them: rub with a pumice stone, or work under the round edge of a blunt knife, to remove the grain, even the thickness and soften the skin.
Bu adım için malzemeler:
Koyun postu12 adet
Sönmüş kireç1 adet
Buğday kepeği1 adetGerekli aletler:
Tabaklama teknesi
Etleme kütüğü
Et alma bıçağı
Ponza taşı4
4
Oil and full
Oil and full
Wring the skins and beat them in the fulling trough until nearly dry. Spread each on the table and sprinkle the grain side with cod or other fish oil, fold them in bundles of four, and beat again 2 to 4 hours. Open and air them briefly, grease again, and full again. Repeat eight or nine times until thoroughly imbued, with no greasy look. 3 to 5 gallons of oil serve a gross of skins. (By hand: beat them in a tub with a heavy wooden mallet, our method.)
Bu adım için malzemeler:
Balık yağı1 adetGerekli aletler:
Tabaklama teknesi
Ahşap Tokmak5
5
Warm and set
Warm and set
Hang the skins on hooks from wooden hangers in a warm drying room (his is about 6 ft high and 12 ft square, heated by steam-pipes or a stove). A slight fermentation sets the oil into the fibre.
6
6
Wash out the excess
Wash out the excess
Handle the skins for an hour in slightly warm potash lye of 2 deg Baume, which turns the excess oil to soap. Wring them at the peg, dry, finish on the stretcher and the stake (horse), and smooth with rollers. For a buff colour dip them in an oak-bark infusion (a dye here, not a tan).
Bu adım için malzemeler:
Potasyum hidroksit1 adet
Meşe kabuğu (kırılmış)1 adetGerekli aletler:
Tabaklama teknesi
20 Litrelik Kova7
7
Troubleshooting
Troubleshooting
Chamois troubleshooting.
Flow
Loading...
8
8
History and honest limits
History and honest limits
From Campbell Morfit, **The Arts of Tanning, Currying, and Leather-Dressing** (1852), "Oiled Leather" (checked on the archive.org scan artsoftanningcur00morf, pp. 433-436). He refers back to kid leather for the pelt stage. Hand fulling, the tools and the diagram are ours.
Malzemeler
6- 12 adetYer Tutucu
- 1 adetYer Tutucu
- 1 adetYer Tutucu
- 1 adetYer Tutucu
- 1 adetYer Tutucu
- 1 adetYer Tutucu
Gerekli Aletler
6- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
Bu planla yapılan
İlgili Blueprint'ler
Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler
CC0 Kamu Malı
Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.
Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.