PETG Pellets: Dimethyl Terephthalate with Ethylene Glycol and CHDM
Charlie

Oluşturan

Charlie

19. Ekim 2026DE
12
0
0
0
0

PETG Pellets: Dimethyl Terephthalate with Ethylene Glycol and CHDM

PETG is PET in which part of the ethylene glycol is replaced by CHDM, which keeps the plastic clear and amorphous. Eastman's patent US 7,026,027 describes PETG 6763 as terephthalate with about 69 mol % ethylene glycol and 31 mol % CHDM, but gives no recipe for it. This blueprint is our own combination: that composition, made by the same patent's pilot-plant process (Example 12, written for a CHDM/neopentyl glycol copolyester), with ethylene glycol in place of neopentyl glycol as in Kibler's 1959 Eastman patent. The charge weights are our arithmetic. The picture: our diagram.
İleri
About 5 hours

Talimatlar

1

Charge the reactor

Our charge for 31 mol % CHDM: 10.669 kg dimethyl terephthalate (54.9 mol, as in the patent's example), 2.456 kg CHDM (31 % of those moles) and 4.058 kg ethylene glycol, so the glycols total 1.5 times the ester moles as in the example. Add 53.4 g of catalyst solution (15 g titanium isopropoxide in 250 ml n-butanol). The patent's reactor held 18 gallons and had spiral agitators and a distillation column.

Bu adım için malzemeler:

Dimetil tereftalatDimetil tereftalat10.669 kg
1,4-Siklohekzandimetanol1,4-Siklohekzandimetanol2.456 kg
Etilen glikolEtilen glikol4.058 kg

Gerekli aletler:

Titanyum izopropoksitTitanyum izopropoksit
n-Butanoln-Butanol
Eşit kollu teraziEşit kollu terazi
Ceketli polimerizasyon reaktörüCeketli polimerizasyon reaktörü
Fraksiyonlu imbikFraksiyonlu imbik
Kimyasal Sıçrama GözlüğüKimyasal Sıçrama Gözlüğü
2

Ester interchange at 200 °C

Stir (forward 50 minutes, then reverse 10), heat to 200 °C and hold 2 hours. Methanol distils off through the column.

Gerekli aletler:

Ceketli polimerizasyon reaktörüCeketli polimerizasyon reaktörü
Fraksiyonlu imbikFraksiyonlu imbik
Göstergeli ısıl çiftGöstergeli ısıl çift
3

260 °C, then 280 °C

Raise to 260 °C for 30 minutes and weigh the distillate, then raise to 280 °C and weigh it again. The surplus ethylene glycol is driven off; Kibler found the CHDM stays in the polymer.

Gerekli aletler:

Ceketli polimerizasyon reaktörüCeketli polimerizasyon reaktörü
Göstergeli ısıl çiftGöstergeli ısıl çift
Eşit kollu teraziEşit kollu terazi
4

Polymerise under vacuum

Switch the agitator direction every 6 minutes and pull vacuum at 13 Torr a minute down to 0.5 Torr. Hold full vacuum for 45 minutes at 25 rpm.

Gerekli aletler:

Ceketli polimerizasyon reaktörüCeketli polimerizasyon reaktörü
Vakum pompasıVakum pompası
Vakum göstergesiVakum göstergesi
Soğuk TuzakSoğuk Tuzak
5

Extrude and chop into pellets

Let nitrogen in, extrude the polymer at once and chop it into pellets. Check the composition: in the patent's example the polymer kept slightly less CHDM than was charged (38.1 % for 40.7 %).

Gerekli aletler:

Azot Gazı TüpüAzot Gazı Tüpü
PeletleyiciPeletleyici
Isıya Dayanıklı EldivenIsıya Dayanıklı Eldiven

Malzemeler

3

Gerekli Aletler

13

CC0 Kamu Malı

Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.

Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.

Tartışma

(0)

Giriş yapın tartışmaya katılmak için

Yorumlar yükleniyor...