İşbirliği
SANAT
GÜZELLİK & SAĞLIK
ZANAAT
KÜLTÜR & TARİH
EĞLENCE
ÇEVRE
YİYECEK & İÇECEK
TERS MÜHENDİSLİK
BİLİMLER
SPOR
TEKNOLOJİ
GİYİLEBİLİR ÜRÜNLER

Semi-Cured Phenolic Sheet: Paper Dipped in Phenol Resin and Part-Cured at 120-130 °C (Lucas, Western Electric, US 1,470,990)
Paper soaked in phenol resin is dried, then cured only part of the way, so the resin is stiff but not yet hard. Lucas did this before the final hot press so the press would not squeeze the resin out of the fibres.
Result: a dry, partly cured phenolic sheet that a later coat of phenolic resin can still bond into.
Source: Lucas, US 1,470,990 (Western Electric, 1923). Stopping before his final hot press is ours. Not given: the solvent in his resin, paper grade, mercerising strengths. Picture drawn by Youblob.
Orta
1 hour
Talimatlar
1
1
Dip the paper in phenol resin
Dip the paper in phenol resin
Run the paper through a bath of phenol resin of specific gravity about 0.970: about 2 minutes for plain paper, 1 minute or less if mercerised first. Ours: Liquid Bakelite as the resin; Lucas does not say how it was thinned.
Bu adım için malzemeler:
Kağıt1 as required
Sıvı bakalit (fenol-formaldehit yoğunlaşma ürünü)1 as requiredGerekli aletler:
Prepreg emdirme hattı
Hidrometre2
2
Optional: mercerise the paper first
Optional: mercerise the paper first
For faster, fuller soaking, first pass the paper through caustic soda, squeeze, wash in water, neutralise in an acid, wash again and dry. Strengths and the acid: not given.
Gerekli aletler:
Sud kostik (sodyum hidroksit)
Prepreg emdirme hattı3
3
Dry at about 90 °C
Dry at about 90 °C
Dry the soaked paper in an oven at about 90 °C, just long enough to dry it.
Gerekli aletler:
Kurutma fırını4
4
Part-cure at 120-130 °C
Part-cure at 120-130 °C
Pass the dry paper through a curing oven at 120-130 °C for about 10 minutes (Lucas's description; his claim 4 says 125 °C for about 10 seconds). The resin sets as stiff as the fibres, but does not harden through.
Gerekli aletler:
Kürleme fırını5
5
Dip again for 10-15 seconds and dry
Dip again for 10-15 seconds and dry
Dip the part-cured paper in phenol resin again for 10-15 seconds, then dry at about 90 °C until it can be wound on a reel. Stop here: the sheet is semi-cured. Lucas's next step, stacking and hot pressing, cures it fully.
Bu adım için malzemeler:
Sıvı bakalit (fenol-formaldehit yoğunlaşma ürünü)1 as requiredGerekli aletler:
Prepreg emdirme hattı
Kurutma fırınıMalzemeler
2- 1 as requiredYer Tutucu
- 1 as requiredYer Tutucu
Gerekli Aletler
5- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
Bu planla yapılan
İlgili Blueprint'ler
Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler