Silver Solder of Silver and Red Copper With a Burnt Wine-Stone Flux (Theophilus, 12th Century)
How Theophilus soldered silver in the 12th century: an alloy of two parts pure silver and a third part red copper, rasped to filings, laid on a joint painted with a flux of burnt wine-stone (tartar) ground with water and salt, and flowed in the coals with a long gentle blast.
Orta
About half a day
Talimatlar
1
1
The alloy
The alloy
Jupyter defteri yükleniyor…
2
2
Read De Diversis Artibus, Book III
Read De Diversis Artibus, Book III
"Weigh two parts of pure silver, and a third (part) of red copper, and mix and finely rasp into a clean vessel."
3
3
Make the solder
Make the solder
Weigh two parts of pure silver and a third part of red copper, melt them together, and rasp the alloy finely into a clean vessel; keep the filings in a quill.
Bu adım için malzemeler:
Saf Gümüş1 adet
Bakır1 adetGerekli aletler:
Eşit kollu terazi
Pota
Pota Maşası
Demirci ocağı
Körük
Törpü
Tüy Kalem4
4
Make the flux
Make the flux
Take wine-stone from a vessel in which good wine has stood a long time, tie pieces in a cloth and put it in the fire until no more vapour comes from it. When cool, blow off the cloth ash and grind the burnt stone in a copper vessel with a round mallet, mixing in water and salt until it is as thick as lees.
Bu adım için malzemeler:
Ham şarap taşı1 adet
Pamuklu Bez1 adet
Tuz1 adetGerekli aletler:
Demirci ocağı
20 Litrelik Kova
Ahşap Tokmak5
5
Solder
Solder
With a thin piece of wood paint the flux round the joint inside and out, shake the filed solder over it with a small iron, and dry it. Paint more flux on, more thickly than before, put the work in the fire, cover it with coals and blow gently with a long breath until the solder has melted. Take it out, let it cool slightly and wash it. If the joint is not firm, do it again. Then file and scrape it smooth.
Gerekli aletler:
Demirci ocağı
Körük
Pota Maşası
Eğeler (El Eğesi)6
6
Troubleshooting
Troubleshooting
Soldering troubleshooting.
Flow
Loading...
7
7
History and honest limits
History and honest limits
From Theophilus, **De Diversis Artibus**, Book III, chapter XXXI, translated by Robert Hendrie (1847) (checked on the archive.org scan essayuponvarious00hend, pp. 241-243). "A third (part)" can be read two ways; both are shown. Melting the alloy before rasping, the tools and the diagram are ours.
Malzemeler
5- 1 adetYer Tutucu
- 1 adetYer Tutucu
- 1 adetYer Tutucu
- 1 adetYer Tutucu
- 1 adetYer Tutucu
Bu planla yapılan
İlgili Blueprint'ler
Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler
CC0 Kamu Malı
Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.
Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.