Metal Oxide Varistor: Zinc Oxide with 0.2 % Bismuth Oxide, Sintered Disc (Masuyama 1972)
A non-linear resistor: the current through it rises far faster than the voltage across it. Masuyama, Matsuoka and Nishi made one from zinc oxide with a little bismuth oxide: pressed into a disc, sintered, lapped, and given metal electrodes. With 0.2 mole % bismuth oxide, sintered at 1000 °C and lapped to 1 mm, the disc measured a C-value of 43 at 1 mA and a nonlinearity exponent n of 4.3.
Source: T. Masuyama, M. Matsuoka and T. Nishi (Matsushita), US 3,663,458 (1972), Example 1. Unknown: how the aluminium is sprayed on and what the silver paint is. The patent calls both well known, so they are linked to unknown heads. The 10 g batch is our arithmetic. Picture: the patent's drawing.
İleri
1 day
Talimatlar
1
1
Weigh 99.8 ZnO to 0.2 Bi2O3 and wet-mill 5 hours
Weigh 99.8 ZnO to 0.2 Bi2O3 and wet-mill 5 hours
Mix zinc oxide and bismuth oxide 99.8 : 0.2 by moles. Ours, for 10 g: 9.887 g zinc oxide and 0.113 g bismuth oxide (our arithmetic). Mill wet for 5 hours, then dry. Unknown: the milling liquid.
Bu adım için malzemeler:
Çinko Oksit Tozu9.887 g
Bizmut oksit0.113 gGerekli aletler:
Eşit kollu terazi
Demir Bilyalı Değirmen
Kurutma fırını2
2
Press discs 13 mm by 2.5 mm
Press discs 13 mm by 2.5 mm
Press the powder in a mould into discs 13 mm across and 2.5 mm thick at 340 kg/cm².
Gerekli aletler:
Hidrolik pres
Disk presleme kalıbı
Kumpas3
3
Sinter 1 hour at 1000 °C and furnace-cool
Sinter 1 hour at 1000 °C and furnace-cool
Sinter the discs in air for 1 hour at 1000 °C, then let them cool in the furnace to room temperature (about 15-30 °C). Above 1200 °C the disc loses its nonlinearity.
Gerekli aletler:
Mufla fırın4
4
Lap both faces to 1.0 mm
Lap both faces to 1.0 mm
Lap both faces with 600-mesh silicon carbide until the disc is 1.0 mm thick.
Gerekli aletler:
Kumpas5
5
Spray aluminium electrodes and attach leads
Spray aluminium electrodes and attach leads
Spray a metallised film of aluminium on both faces. Attach a lead wire to each with conductive silver paint. Unknown: the spraying method and the paint.
Bu adım için malzemeler:
Alüminyum külçe1 as required
Gümüş iletken boya1 as required
Bakır Tel2 adetGerekli aletler:
Bilinmeyen metal püskürtme yöntemi
KumpasMalzemeler
5- 9.887 gYer Tutucu
- 0.113 gYer Tutucu
- 1 as requiredYer Tutucu
- 1 as requiredYer Tutucu
- 2 adetYer Tutucu
Gerekli Aletler
9- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
- Yer Tutucu
Bu planla yapılan
İlgili Blueprint'ler
Bu blueprint'ler bilgi paylaşır — teknikler, malzemeler veya ilkeler
CC0 Kamu Malı
Bu plan CC0 lisansıyla yayınlanmıştır. İzin almadan kopyalayabilir, değiştirebilir, dağıtabilir ve herhangi bir amaçla kullanabilirsiniz.
Planı üzerinden ürün satın alarak Maker'ı destekleyin, böylece Maker Komisyonu Satıcılar tarafından belirlenen komisyonu kazanırlar veya bu Planın yeni bir versiyonunu oluşturun ve gelir paylaşımı için kendi Planınıza bağlantı olarak ekleyin.