Carbon Film Resistors: Methane Cracked on Ceramic Rods, Helixed and Varnished (Bell Labs 1951)
Ed

Створено

Ed

2. листопад 2026FI
10
0
0
0
0

Carbon Film Resistors: Methane Cracked on Ceramic Rods, Helixed and Varnished (Bell Labs 1951)

Ceramic rods tumble in a hot, gas-tight rotating furnace while methane cracks on them and leaves a thin, hard film of carbon. The coated rods get conducting ends, a helix ground through the film to bring them near their value, a light rub to the exact value, and a coat of baking varnish. Result: carbon film resistors adjusted to as close as ±0.5 %. The helix alone can raise a rod's resistance by any factor from about 10 to about 8000. Source: Grisdale, Pfister and van Roosbroeck, Pyrolytic Film Resistors, Bell System Technical Journal 30 (1951). Unknown: the ceramic of the rods, the end caps and leads, and which baking varnish; the paper does not give them. Picture: Wikimedia Commons.
Просунутий
2 days

Інструкції

1

Load the furnace

Load cylindrical ceramic rods into the gas-tight refractory core of a rotating (or rocking) batch furnace, with silica sand to support the rods and keep them from damage as they tumble. Unknown: which ceramic.

Матеріали для цього кроку:

Ізоляційне осердя резистораІзоляційне осердя резистора1 batch

Необхідні інструменти ({count})

Обертова періодична пічОбертова періодична піч
Кварцовий пісокКварцовий пісок
2

Heat under nitrogen

Turn the core and bring it to temperature, usually about 975 to 1300 °C, flushing it with nitrogen before any hydrocarbon goes in.

Необхідні інструменти ({count})

Обертова періодична пічОбертова періодична піч
АзотАзот
3

Crack the methane

When the temperature is steady, let in the coating gas and keep it flowing for the time needed. The film grows at a steady rate: at 1000 °C and 30 % methane the paper runs from 0.2 to 10 hours. Longer gives a thicker film of lower resistance; temperature sets the rate more than anything else, and more methane deposits faster.

Матеріали для цього кроку:

МетанМетан1 flow

Необхідні інструменти ({count})

Обертова періодична пічОбертова періодична піч
4

Cool under nitrogen

Shut off the methane and let the core cool while oxygen-free nitrogen keeps flowing. The films come out clean, even and firmly stuck.

Необхідні інструменти ({count})

Обертова періодична пічОбертова періодична піч
АзотАзот
5

Terminate the ends

Paint the ends of each coated rod with a water suspension of colloidal graphite (Aquadag), then burnish and bake it; this suits all but low-value resistors. Fit the end caps with their leads. Unknown: the caps and leads, which the paper does not describe. Ours: an agate burnisher and an oven.

Матеріали для цього кроку:

Колоїдний графітКолоїдний графіт1 as required
Ковпачки резистора з виводамиКовпачки резистора з виводами2 per resistor

Необхідні інструменти ({count})

Агатове гладилоАгатове гладило
ДуховкаДуховка
6

Grind the helix

Grind a helical groove through the film with a water-cooled, metal-bonded diamond wheel, the blank floating against the wheel so the groove stays even. Pick the pitch to land slightly below the wanted value (330 Ω, 10 kΩ or any other). The groove must be smooth: cracks into the carbon ribbon bring noise and drift.

Необхідні інструменти ({count})

Верстат для нарізання спіралі резисторівВерстат для нарізання спіралі резисторів
7

Rub to value and varnish

Turn the resistor while measuring it continuously, and rub its whole surface lightly with a cotton pad wet with an organic solvent until it reaches its value. Leave it just below tolerance, then give it one or more coats of baking varnish, which raises the resistance by generally less than 1 %. Unknown: which varnish and its baking. Ours: acetone as the solvent, a Wheatstone bridge to measure.

Матеріали для цього кроку:

Пічний лакПічний лак1 as required

Необхідні інструменти ({count})

Міст ВітстонаМіст Вітстона
Вата гігроскопічнаВата гігроскопічна
АцетонАцетон
ДуховкаДуховка

Матеріали

5

Необхідні інструменти

9

Пов'язані креслення

Ці креслення діляться знаннями — техніки, матеріали або принципи

CC0 Суспільне надбання

Це креслення випущено під ліцензією CC0. Ви можете вільно копіювати, змінювати, поширювати та використовувати цю роботу для будь-яких цілей без запиту дозволу.

Підтримайте мейкера, купуючи продукти через його креслення, де він отримує Комісію мейкера встановлену вендорами, або створіть нову ітерацію цього креслення та включіть його як зв'язок у власне креслення для розподілу доходу.

Обговорення

(0)

Увійти щоб приєднатися до обговорення

Завантаження коментарів...