Black Cobbler's Wax: Resin and Pitch With Linseed Oil, Pulled to Golden Colour (Hasluck, Harness Making, 1904)
Forge

Створено

Forge

14. листопад 2026NO
7
0
0
0
0

Black Cobbler's Wax: Resin and Pitch With Linseed Oil, Pulled to Golden Colour (Hasluck, Harness Making, 1904)

The saddler's black wax for waxed threads, from P. N. Hasluck's Harness Making (1904): half a pound each of resin and pitch melted together, softened with boiled linseed oil to suit the season, poured into cold water and pulled by wet hands until golden and until a piece floats. It makes about thirty lumps, kept under water.
Початківець
About 1 hour

Інструкції

1

Batch in grams

Завантаження блокнота Jupyter…
2

Read Harness Making

"Black cobbler's wax is made by melting together 1/2 lb. each of resin and pitch."
3

Melt and oil

Melt 1/2 lb of resin and 1/2 lb of pitch together and mix thoroughly. Take the pan off the fire and add boiled linseed oil, about a pennyworth or less: only half as much in summer as in winter, more the colder it is. Mix well.

Матеріали для цього кроку:

Соснова живицяСоснова живиця1 штука
Деревний дігтярний пекДеревний дігтярний пек1 штука
Варена лляна оліяВарена лляна олія1 штука

Необхідні інструменти ({count})

Велика каструляВелика каструля
Пропановий пальникПропановий пальник
Важільні терезиВажільні терези
4

Test

Pour a little into cold water, leave it a minute, and take it out with well-wetted hands. If it cracks when worked it is too hard; if it pulls out and sticks together it is right. Do not put the tested piece back in the pan: the water in it froths the hot wax.

Необхідні інструменти ({count})

Відро на 20 літрівВідро на 20 літрів
5

Pour and pull

Put the test piece back in the water and pour the rest in after it. Gather the wax with wet hands without delay and pull it fast, hand over hand, until it is a light golden colour. Cut off a piece with wet scissors and drop it in the water: if it floats it has been pulled enough; if it sinks, pull more. Under-pulled wax is brittle.

Необхідні інструменти ({count})

Відро на 20 літрівВідро на 20 літрів
НожиціНожиці
6

Adjust and store

If it is too hard, melt again and add oil; if too soft, add pitch and resin. Cut it into lumps the size of a large pigeon's egg (about thirty) and keep them in water.

Необхідні інструменти ({count})

НожиціНожиці
Відро на 20 літрівВідро на 20 літрів
7

Troubleshooting

Wax troubleshooting.

Flow

Loading...
8

History and honest limits

From Paul N. Hasluck, **Harness Making** (1904), "Harness-makers' Materials" (checked on the archive.org scan harnessmaking00hasl, pp. 30-31). He says only "pitch"; wood-tar pitch is our choice. His white wax, made with white lead, is left out because white lead is a poison. The metric figures and the diagram are ours.

Матеріали

3

Необхідні інструменти

5

За цим кресленням виготовляють

Пов'язані креслення

Ці креслення діляться знаннями — техніки, матеріали або принципи

CC0 Суспільне надбання

Це креслення випущено під ліцензією CC0. Ви можете вільно копіювати, змінювати, поширювати та використовувати цю роботу для будь-яких цілей без запиту дозволу.

Підтримайте мейкера, купуючи продукти через його креслення, де він отримує Комісію мейкера встановлену вендорами, або створіть нову ітерацію цього креслення та включіть його як зв'язок у власне креслення для розподілу доходу.

Обговорення

(0)

Увійти щоб приєднатися до обговорення

Завантаження коментарів...