Hydroxyl-Ended Silicone Oil: D4 Opened with Potash, Then Water (Ceyzeriat 1964)
Youblob · CC0
Charlie

Створено

Charlie

27. жовтень 2026DE
7
0
0
0
0

Hydroxyl-Ended Silicone Oil: D4 Opened with Potash, Then Water (Ceyzeriat 1964)

A trace of hot potash opens the ring of D4 and strings it into a long, thick chain. Water added a little at a time then cuts the chains back and leaves hydroxyl groups on their ends, which is what later lets the oil cure into rubber. This is Louis Ceyzeriat's oil A, the base of every sealant in his patent: 21,000 centistokes, 0.15 % hydroxyl. Source: L. Ceyzeriat (Rhône-Poulenc), US 3,133,891 (1964), column 4. His neutraliser was the precipitated silica Hi-Sil X303; we use our precipitated silica in its place. The potash mix and the equipment are ours. Picture drawn by Youblob.
Просунутий
2 days

Інструкції

1

Make the 10 % potash

Dissolve 0.5 part of potassium hydroxide in 4.5 parts of water (our arithmetic for 5 parts of a 10 % solution). All parts are by weight.

Матеріали для цього кроку:

Гідроксид каліюГідроксид калію0.5 parts
ВодаВода4.5 parts

Необхідні інструменти ({count})

Скляна посудинаСкляна посудина
Важільні терезиВажільні терези
2

Heat D4 with the potash under nitrogen

Heat 5000 parts of octamethylcyclotetrasiloxane (it melts at 17.5 °C) with the 5 parts of 10 % potash at 150 °C for 3½ hours under nitrogen. The oil thickens to 31,000 centistokes while hot.

Матеріали для цього кроку:

Октаметилциклотетрасилоксан (D4)Октаметилциклотетрасилоксан (D4)5000 parts

Необхідні інструменти ({count})

Скляна перегінна колбаСкляна перегінна колба
ЕлектроплиткаЕлектроплитка
ТермометрТермометр
МішалкаМішалка
Балон з азотомБалон з азотом
3

Add water a little at a time

Still hot, add 16.5 parts of water in small portions over 3 hours 40 minutes. The hot oil thins to 1730 centistokes.

Матеріали для цього кроку:

ВодаВода16.5 parts

Необхідні інструменти ({count})

Скляна перегінна колбаСкляна перегінна колба
ЕлектроплиткаЕлектроплитка
ТермометрТермометр
МішалкаМішалка
4

Cool, then neutralise with silica

Let it cool for 15 hours. Then stir in 50 parts of precipitated silica to neutralise the potash. The liquid now measures 13,400 centistokes at 25 °C.

Матеріали для цього кроку:

Осаджений кремнеземОсаджений кремнезем50 parts

Необхідні інструменти ({count})

Скляна перегінна колбаСкляна перегінна колба
МішалкаМішалка
5

Strip the volatiles at 195–200 °C

Heat it to about 195–200 °C in a current of nitrogen, with a water condenser on the outlet. 655 parts of liquid distil over; 4345 parts of oil A stay in the boiler, 21,000 centistokes at 25 °C with 0.15 % hydroxyl groups.

Необхідні інструменти ({count})

Скляна перегінна колбаСкляна перегінна колба
Змійовик конденсатораЗмійовик конденсатора
ЕлектроплиткаЕлектроплитка
ТермометрТермометр
Балон з азотомБалон з азотом
Скляна банка з кришкоюСкляна банка з кришкою

Матеріали

4

Необхідні інструменти

9

CC0 Суспільне надбання

Це креслення випущено під ліцензією CC0. Ви можете вільно копіювати, змінювати, поширювати та використовувати цю роботу для будь-яких цілей без запиту дозволу.

Підтримайте мейкера, купуючи продукти через його креслення, де він отримує Комісію мейкера встановлену вендорами, або створіть нову ітерацію цього креслення та включіть його як зв'язок у власне креслення для розподілу доходу.

Обговорення

(0)

Увійти щоб приєднатися до обговорення

Завантаження коментарів...