Neodymium Magnets, Sample 12: 55Fe-30B-15Nd Sintered (Sagawa 1988)
Neodymium magnets are iron, boron and neodymium. Sagawa's team at Sumitomo melted the three together, ground the casting to a powder finer than 10 µm, lined the grains up in a magnetic field while pressing them, and sintered the compact in argon. This is their sample 12, 55 % iron, 30 % boron and 15 % neodymium by atoms: 4.0 MGOe.
Source: M. Sagawa et al. (Sumitomo Special Metals), US 4,770,723 (1988). Unknown: how the pure iron, the ferroboron and the neodymium metal are made, and how the finished magnets are magnetised; the patent does not say. The 1 kg weights are our arithmetic from the patent's atomic percentages. Picture: the patent's Fig. 8.
Експерт
2 days
Інструкції
1
1
Weigh sample 12: 55 Fe, 30 B, 15 Nd
Weigh sample 12: 55 Fe, 30 B, 15 Nd
Sample 12 is 55 % iron, 30 % boron and 15 % neodymium by atoms. Use 99.9 % electrolytic iron, ferroboron (19.38 % B, 5.32 % Al, 0.74 % Si, 0.03 % C, the rest iron) and neodymium of 99.7 % or better. Ours: a 1 kg melt, by arithmetic: 328.1 g iron, 301.0 g ferroboron, 389.2 g neodymium. Unknown: how these three are made.
Матеріали для цього кроку:
Електролітичне залізо328.1 г
Феробор301 г
Металевий неодим389.2 гНеобхідні інструменти ({count})
Важільні терези2
2
Melt by high frequency in argon and cast
Melt by high frequency in argon and cast
Melt the charge in a high-frequency (induction) furnace under argon and pour it into a water-cooled copper mould.
Необхідні інструменти ({count})
Індукційна піч
Тигель із вогнетривкої глини
Аргон
Балон для газу під тиском
Водоохолоджувана мідна виливниця
Термостійкі рукавиці3
3
Stamp to 35 mesh, ball-mill to 3-10 µm
Stamp to 35 mesh, ball-mill to 3-10 µm
Crush the casting in a stamp mill until it passes a 35-mesh sieve. Then grind it in a ball mill for 3 hours, to 3-10 µm.
Необхідні інструменти ({count})
Товчильний млин
Набір сит (ступінчасте вічко)
Залізний кульовий млин
Захисні окуляри4
4
Press in a 10 kOe field at 1.5 t/cm²
Press in a 10 kOe field at 1.5 t/cm²
Line the powder up in a magnetic field of 10 kOe and press it at 1.5 tonnes per cm². Unknown: the size and shape of the magnets.
Необхідні інструменти ({count})
Прес із магнітним полем5
5
Sinter in argon at 1000-1200 °C
Sinter in argon at 1000-1200 °C
Sinter the compacts at 1000-1200 °C for about one hour in argon, then let them cool. Sample 12 measured 4.2 kG remanence, 10.7 kOe coercivity and 4.0 MGOe.
Необхідні інструменти ({count})
Трубчаста піч
Аргон
Балон для газу під тиском
Термостійкі рукавиці6
6
Magnetise the magnets
Magnetise the magnets
Unknown: how the sintered magnets are magnetised. Sagawa measures them on a B-H tracer but gives no magnetising field or apparatus.
Необхідні інструменти ({count})
Невідомий спосіб намагнічуванняМатеріали
3- 328.1 гЗаповнювач
- 301 гЗаповнювач
- 389.2 гЗаповнювач
Необхідні інструменти
14- Заповнювач
- Заповнювач
- Заповнювач
- Заповнювач
- Заповнювач
- Заповнювач
- Заповнювач
- Заповнювач
- Заповнювач
- Заповнювач
- Заповнювач
- Заповнювач
- Заповнювач
- Заповнювач
За цим кресленням виготовляють
Пов'язані креслення
Ці креслення діляться знаннями — техніки, матеріали або принципи
CC0 Суспільне надбання
Це креслення випущено під ліцензією CC0. Ви можете вільно копіювати, змінювати, поширювати та використовувати цю роботу для будь-яких цілей без запиту дозволу.
Підтримайте мейкера, купуючи продукти через його креслення, де він отримує Комісію мейкера встановлену вендорами, або створіть нову ітерацію цього креслення та включіть його як зв'язок у власне креслення для розподілу доходу.