Swedish Bar Iron: White Pig Iron Refined in a Walloon Finery and Drawn under Water Hammers, as at Dannemora (Percy, 1864)
Forge

Створено

Forge

1. листопад 2026NO
9
0
0
0
0

Swedish Bar Iron: White Pig Iron Refined in a Walloon Finery and Drawn under Water Hammers, as at Dannemora (Percy, 1864)

The renowned bar iron of Dannemora was refined in the old Walloon way: long white pigs melt drop by drop before a cold blast in a small, very hot charcoal hearth, the finer works the metal with an iron staff until it comes to nature, and the lump is drawn out under water-driven hammers. Result: bars 12 ft long of about 60 lb; 6 tons a week from one hearth, 80 % of the weight of the pig. Source: John Percy, Metallurgy: Iron and Steel (1864), pp. 599-601, after Tunner and A. Grill. Picture drawn by Youblob.
Експерт
about 30 minutes per lump; 8-hour shifts

Інструкції

1

Build the finery hearth

Make the hearth of cast-iron plates: a 2-inch bottom plate on about 3 inches of pounded slag, over a cast-iron box with channels to drain water. From the tuyere it is 10-11½ inches to the back-plate, 22-24 inches to the work-plate and 22-24 inches to the opposite side. Depth: 7-8 inches under the tuyere, 14-15 under the back-plate, 15-18 opposite the tuyere. No tapping hole: the slag is never let out.

Необхідні інструменти ({count})

Кричний горнКричний горн
2

Set the tuyere and blast

The tuyere nozzle is semicircular, flat side down, 20-25 lines broad and 16-17 lines high, and projects 3½ inches; the blast-pipe nozzle sits 4 inches back inside it. Use cold blast. The blowing machine is not described.

Необхідні інструменти ({count})

Кричний горнКричний горн
Ковальський міхКовальський міх
3

Lay in the pigs

Use white or strongly mottled pig in long pigs about 9 inches broad, 15-18 feet long, 3-4 inches thick at one end and 1-2 at the other. Lay them across the back-plate, one end sloping down over the tuyere, usually two one above the other, and push them forward as the ends melt.

Матеріали для цього кроку:

Білий деревновугільний чавунБілий деревновугільний чавун1 long pigs

Необхідні інструменти ({count})

Кричний горнКричний горн
4

Light and make the slag bath

Fill the front of the hearth with moistened small charcoal and the rest with charcoal, light it and turn on the blast. To make enough slag bath, melt down some large finery scraps or, failing these, several shovelfuls of hammer scale.

Необхідні інструменти ({count})

Деревне вугілля — дрібного помелуДеревне вугілля — дрібного помелу
ВодаВода
Деревне вугілляДеревне вугілля
Кувальна окалинаКувальна окалина
ЛопатаЛопата
5

Reheat the last bloom

At the start of each heat, hold the bloom from the last lump with tongs, as steeply as you can, in the front of the hearth to reheat it for drawing out.

Необхідні інструменти ({count})

Ковальські кліщіКовальські кліщі
6

Work the metal with the staff

As soon as the first pig iron melts, work it with an iron staff: bring the metal on the tuyere side up from the bottom towards the middle into the blast, once to the left and once to the right of the reheating bloom. About 70 lb melts in 20 minutes; thin pieces of malleable iron then cling to the staff.

Необхідні інструменти ({count})

Круглий залізний прутокКруглий залізний пруток
7

Form the lump

Stop the flow of fresh molten pig, break up all the metal above the tuyere, melt it down and gather it into a lump about 12 by 15 inches. One lump takes 28 minutes on average (25-30).

Необхідні інструменти ({count})

Круглий залізний прутокКруглий залізний пруток
Ковальські кліщіКовальські кліщі
8

Draw out the bar

Heat each lump 6-8 times in a separate fire and draw it out under water-driven hammers into a bar 12 feet long of about 60 lb. One finery, one drawing-out forge and one hammer make 6 tons of bars a week; the bars weigh 80 % of the pig, and take 3 tons of charcoal per ton.

Необхідні інструменти ({count})

ГорноГорно
Хвостовий молотХвостовий молот
Водяне колесоВодяне колесо
Ковальські кліщіКовальські кліщі

Матеріали

1

Необхідні інструменти

12

За цим кресленням виготовляють

CC0 Суспільне надбання

Це креслення випущено під ліцензією CC0. Ви можете вільно копіювати, змінювати, поширювати та використовувати цю роботу для будь-яких цілей без запиту дозволу.

Підтримайте мейкера, купуючи продукти через його креслення, де він отримує Комісію мейкера встановлену вендорами, або створіть нову ітерацію цього креслення та включіть його як зв'язок у власне креслення для розподілу доходу.

Обговорення

(0)

Увійти щоб приєднатися до обговорення

Завантаження коментарів...