Barium Sulphide: Heavy Spar Roasted with Coal
Barium sulphide is the barium half of lithopone, the white pigment. Thorpe (1912): roast 100 parts of heavy spar with 20 parts of coal slack or charcoal. Caking bituminous coal soaks through the mass and reduces it completely; with charcoal, mix very thoroughly. The roasted mass still holds carbon and some unchanged spar: hot water takes out the barium sulphide. Left in air it turns to carbonate and smells of rotten eggs, so keep it closed.
The picture: our own drawing.
Intermediate
1 day
Instructions
1
1
Grind and mix
Grind and mix
Grind 100 g of heavy spar and 20 g of bituminous coal slack and mix them very thoroughly.
Materials for this step:
Barite (Heavy Spar)100 gTools needed:
Bituminous Coal
Mortar and Pestle
Balance Scale2
2
Roast
Roast
Roast the mixture in a crucible in the furnace. The coal cakes and runs through the mass, reducing the spar.
Tools needed:
Clay Crucible - Deep
Charcoal Furnace
Leather Gloves3
3
Cool and close it up
Cool and close it up
Let it cool and put it straight into an airtight jar. It holds spare carbon and some unchanged spar; hot water dissolves out the barium sulphide when you use it.
Tools needed:
Dark Glass Jars with Airtight Lids
Leather GlovesMaterials
1- 100 gPlaceholder
Tools Required
7- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
- Placeholder
This blueprint makes
CC0 Public Domain
This blueprint is released under CC0. You are free to copy, modify, distribute, and use this work for any purpose, without asking permission.
Support the Maker by purchasing products through their Blueprint where they earn a Maker Commission set by Vendors, or create a new iteration of this Blueprint and include it as a connection in your own Blueprint to share revenue.