Acrylic Block: Methyl Methacrylate Syrup Cast in Layers between Glass
A thick acrylic block cannot be cast flawless in one pour. Tattersall (ICI, US 2,071,907, 1937) built it up in layers: pour 1/2 inch of syrup on a level glass plate, let it set for a day at room temperature, pour the next 1/2 inch on top, cover with a second glass plate, wait another day, then heat the sandwich at 80 °C. Each 1/2 inch layer shrinks to about 1/3 inch. The glass gives both faces a finished polish with no grinding.
The picture: our diagram.
Trung cấp
3 days
Hướng dẫn
1
1
Level the bottom plate
Level the bottom plate
Set a glass plate on a ledge in a wooden frame, on a body of plaster of Paris, and level it carefully. The example sheet was 10 by 18 inches.
Công cụ cần thiết:
Tấm kính
Khung gỗ
Thạch cao Paris
Nivô 1,5 m2
2
Pour the first 1/2 inch
Pour the first 1/2 inch
Pour room-temperature syrup 1/2 inch deep (about 1.5 litres for 10 by 18 inches; our figure). Cover against dust, but do not put the top plate on yet. Leave 24 hours at about 20 °C.
Vật liệu cho bước này:
Siro metyl metacrylat3 lCông cụ cần thiết:
Găng tay cao su
Nhiệt kế phòng thí nghiệm3
3
Pour the next layer and cover
Pour the next layer and cover
Pour a second 1/2 inch layer on the first. Lower the top glass plate onto it so it rests on the syrup and keeps pressing on it. Leave another 24 hours at about 20 °C. For a thicker block repeat the layers, a day apart, and put the plate on the last one.
Công cụ cần thiết:
Tấm kính4
4
Heat at 80 °C
Heat at 80 °C
Take the glass sandwich out of the frame and heat it for three hours at 80 °C to finish the polymerisation.
Công cụ cần thiết:
Lò sấy
Nhiệt kế phòng thí nghiệm
Găng tay chịu nhiệt5
5
Spring off the glass
Spring off the glass
Spring the glass plates off the block with a knife blade. Both faces come out smooth and polished.
Công cụ cần thiết:
Dao rọc thủ công
Găng tay cao suVật liệu
1- Tạm thời
Bản thiết kế này làm ra
Blueprint liên quan
Các blueprint này chia sẻ kiến thức — kỹ thuật, vật liệu hoặc nguyên tắc
CC0 Phạm vi công cộng
Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.
Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.