The dark grey ceramic magnet on fridges and in loudspeakers is barium ferrite. It is made from two cheap powders: one part barium carbonate to six of iron oxide, milled, fired, milled again, pressed and sintered. No cobalt or nickel is needed. This is Example 34 of the Philips patent. Fired 4 hours at 1100 °C, its rod held 1,375 gauss with a coercive force of 3,350 oersted.
Source: J. J. Went, G. W. van Oosterhout and E. W. Gorter (Philips), US 2,762,777 (1956). They pressed rods; the claim covers "a body of a desired shape", and the disc size is ours. The patent does not say how to magnetise it; our way is stated. Picture: ferrite magnets, Omegatron, Wikimedia Commons, CC BY-SA 3.0.
Nâng cao
2 days
Hướng dẫn
1
1
Weigh one part barium carbonate to six of iron oxide
Weigh one part barium carbonate to six of iron oxide
Weigh 39.5 g of barium carbonate (0.2 mol) and 191.7 g of ferric oxide, Fe2O3 (1.2 mol). Barium carbonate is poisonous if swallowed: ours, gloves and a dust respirator.
Vật liệu cho bước này:
Bari cacbonat (witherit)39.5 g
Oxit sắt(III)191.7 gCông cụ cần thiết:
Cân hai đĩa
Găng tay cao su
Mặt nạ phòng độc P1002
2
Mill with ethanol for 4 hours
Mill with ethanol for 4 hours
Grind the mixture with ethanol in an iron ball mill for 4 hours. Let the ethanol evaporate, then dry the powder in a drying oven.
Công cụ cần thiết:
Máy nghiền bi sắt
Etanol phẩm cấp thí nghiệm, 95 %
Lò sấy3
3
Presinter at 1000 °C for 4 hours
Presinter at 1000 °C for 4 hours
Fire the dry powder in air at 1000 °C for 4 hours (ours: in a lidded porcelain crucible in a muffle furnace). Let it cool.
Công cụ cần thiết:
Lò muffle
Chén nung có nắp (sứ)
Kìm gắp nồi nấu kim loại
Găng tay chịu nhiệt4
4
Mill again for 4 hours
Mill again for 4 hours
Grind the presintered product with ethanol in the ball mill for another 4 hours. Let the ethanol evaporate.
Công cụ cần thiết:
Máy nghiền bi sắt
Etanol phẩm cấp thí nghiệm, 95 %
Lò sấy
Mặt nạ phòng độc P1005
5
Press discs at 1.5 tons per cm²
Press discs at 1.5 tons per cm²
Press the powder at 1.5 tons/cm². The patent pressed rods; we press discs. Ours: a die 20 mm across, so about 4.7 tonnes on the punch (our arithmetic: 1.5 × 3.14 cm²).
Công cụ cần thiết:
Máy ép thủy lực
Khuôn ép đĩa6
6
Sinter for 4 hours
Sinter for 4 hours
Sinter the discs for 4 hours in oxygen or in air. The patent's results: at 1100 °C, 1,375 gauss and 3,350 oersted; at 1200 °C, 1,400 and 3,100; at 1300 °C, 1,850 and 1,780. Hotter gives a stronger but less stubborn magnet.
Công cụ cần thiết:
Lò muffle
Kìm gắp nồi nấu kim loại
Găng tay chịu nhiệt7
7
Magnetise the discs
Magnetise the discs
The patent gives no magnetising method. Ours: lay a disc with its faces against the poles of a strong electromagnet, switch the current on, then off. Find which face is north with a compass.
Công cụ cần thiết:
Nam châm điện
La bànVật liệu
2- 39.5 gTạm thời
- 191.7 gTạm thời
Công cụ yêu cầu
14- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
Bản thiết kế này làm ra
Blueprint liên quan
Các blueprint này chia sẻ kiến thức — kỹ thuật, vật liệu hoặc nguyên tắc
CC0 Phạm vi công cộng
Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.
Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.