Mallory's quiet volume-control ring (US 2,144,925, 1939). Hard bases were noisy and soft paper ones changed with damp. Their answer: paper rings soaked in 15 % raw tung oil and baked, so the oil gels inside the paper. It shuts out moisture but stays soft and springy, and the wiper runs on it quietly. A graphite paint makes the track, silver paint the ends.
The picture: the patent's drawing (Fig. 3).
Trung cấp
1 day
Hướng dẫn
1
1
Punch rings from three-ply paper
Punch rings from three-ply paper
The base is three papers stuck into one sheet: litho paper at the back, newsprint in the middle, manila on the face that takes the track. Punch rings from it. Ours: a punch press with a ring die.
Vật liệu cho bước này:
Giấy ép ba lớp1 cáiCông cụ cần thiết:
Máy đột dập
Khuôn dập vòng
Găng tay cao su2
2
Soak 1 hour in 15 % tung oil in naphtha
Soak 1 hour in 15 % tung oil in naphtha
Soak the rings for about one hour in about 15 % raw tung oil in naphtha. Use raw oil, not heat-bodied or treated oil, so it can still gel.
Vật liệu cho bước này:
Dầu trẩu15 partsCông cụ cần thiết:
Naphta
Cốc thủy tinh (becher)
Cân hai đĩa
Que khuấy
Mặt nạ phòng độc toàn mặt
Găng tay cao su3
3
Air-dry, then bake at 210–250 °C
Air-dry, then bake at 210–250 °C
Dry the rings in air for two hours or more, then bake 15 to 30 minutes at 210 to 250 °C. The oil gels in the paper's pores; the paper stays pliable.
Công cụ cần thiết:
Lò sấy
Nhiệt kế lò nướng
Găng tay chịu nhiệt4
4
Spray the graphite track
Spray the graphite track
Spray on the resistance paint, for example graphite in a shellac binder. The patent gives no proportions. The track can be tapered in thickness, width or mix to shape the resistance curve.
Vật liệu cho bước này:
Bột than chì1 as required
Cánh kiến1 as requiredCông cụ cần thiết:
Súng phun
Máy nén khí
Mặt nạ phòng độc toàn mặt
Găng tay cao su5
5
Paint silver ends, bake at 220 °C
Paint silver ends, bake at 220 °C
Spray or paint the two end terminals with silver particles in shellac. Dry, then bake at about 220 °C to cure and harden the track. The slight warp from soaking flattens out again.
Vật liệu cho bước này:
Sơn bạc dẫn điện1 as requiredCông cụ cần thiết:
Súng phun
Lò sấy
Nhiệt kế lò nướng
Găng tay chịu nhiệtVật liệu
5- 1 cáiTạm thời
- 15 partsTạm thời
- 1 as requiredTạm thời
- 1 as requiredTạm thời
- 1 as requiredTạm thời
Công cụ yêu cầu
13- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- 1 vendor sell this, none ship to you yetTạm thời
Bản thiết kế này làm ra
Blueprint liên quan
Các blueprint này chia sẻ kiến thức — kỹ thuật, vật liệu hoặc nguyên tắc
CC0 Phạm vi công cộng
Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.
Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.