Carbon Resistance Strip: Carbon and Phenolic Resin in Acetone, Cured on Semi-Cured Phenolic Sheet

Podolsky (Wirt Company, US 2,060,114, 1936) bonded the carbon film into its base: the phenolic sheet is only half cured, the coating carries the same kind of resin, and its solvent (acetone) softens the sheet's surface. Heated calender rolls then finish the cure of sheet and coating together, so the track is hard, does not rub off and lasts. Cut across, the sheet gives resistance strips for a variable resistor. The picture: our diagram.
Trung cấp
1 day

Hướng dẫn

1

Mix 21 carbon, 26 resin, 53 solvent

Make a solution of 21 % carbon, 26 % phenol-formaldehyde resin and 53 % acetone. The patent says the exact proportions are not essential; this is its example.

Vật liệu cho bước này:

CacbonCacbon21 parts
Bakelite lỏng (sản phẩm ngưng tụ phenol-formaldehyde)Bakelite lỏng (sản phẩm ngưng tụ phenol-formaldehyde)26 parts

Công cụ cần thiết:

AxetonAxeton
Cân hai đĩaCân hai đĩa
Cốc thủy tinh (becher)Cốc thủy tinh (becher)
Que khuấyQue khuấy
Mặt nạ phòng độc toàn mặtMặt nạ phòng độc toàn mặt
Găng tay cao suGăng tay cao su
2

Coat the semi-cured sheet

Use a phenolic sheet whose cure was stopped before it fully hardened. A roller turning in a pan of the solution coats its underside.

Vật liệu cho bước này:

Tấm phenolic bán đóng rắnTấm phenolic bán đóng rắn1 cái

Công cụ cần thiết:

Cặp trục lăn phủ nhúngCặp trục lăn phủ nhúng
Mặt nạ phòng độc toàn mặtMặt nạ phòng độc toàn mặt
Găng tay cao suGăng tay cao su
3

Cure between calender rolls at 350 °F

Pass the coated sheet between calender rolls heated to about 350 °F (177 °C). This finishes the cure and bonds the coating to the sheet. The patent sometimes calenders it again to burnish the surface.

Công cụ cần thiết:

Cặp trục cán nóngCặp trục cán nóng
Găng tay chịu nhiệtGăng tay chịu nhiệt
4

Cut into strips

Cut the sheet across into strips of the width wanted. Ours: tin snips.

Công cụ cần thiết:

Kéo cắt tônKéo cắt tôn
Găng tay cao suGăng tay cao su

Vật liệu

3

Công cụ yêu cầu

10

CC0 Phạm vi công cộng

Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.

Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.

Thảo luận

(0)

Đăng nhập để tham gia thảo luận

Đang tải bình luận...