Chromium Metal: Chromic Oxide Reduced by Aluminium (Thermit)
Forge

Tạo bởi

Forge

18. tháng Mười 2026NO
17
0
0
0
0

Chromium Metal: Chromic Oxide Reduced by Aluminium (Thermit)

Aluminium takes the oxygen from chromic oxide with so much heat that the chromium comes out molten. Thorpe (1912-13) gives Goldschmidt's thermit: chromic oxide mixed with aluminium powder in a magnesia-lined crucible, lit through a fuse of aluminium powder and barium peroxide with a magnesium ribbon. The heat carries the reaction through the whole charge, and carbon-free chromium sinks under a slag of alumina. White heat: outdoors on dry sand, face shield, stand well back. The picture: chromium metal (Wikimedia Commons).
Nâng cao
1 day

Hướng dẫn

1

Line the crucible

Line a refractory crucible with a paste of magnesia and water glass, and let it dry fully.

Công cụ cần thiết:

Nồi nấu bằng đất chịu lửaNồi nấu bằng đất chịu lửa
Magiê oxitMagiê oxit
Thủy tinh lỏng (dung dịch natri silicat)Thủy tinh lỏng (dung dịch natri silicat)
2

Mix the charge

Weigh 150 g of dry chromic oxide and 50 g of aluminium powder, a little less than the 53 g the equation needs, and mix them intimately.

Vật liệu cho bước này:

Oxit cromOxit crom150 g
Bột nhômBột nhôm50 g

Công cụ cần thiết:

Cân hai đĩaCân hai đĩa
Cối và chàyCối và chày
3

Set the fuse

Stand the crucible on dry sand outdoors and fill in the charge. On top put a small heap of aluminium powder mixed with barium peroxide, and push a strip of magnesium ribbon into it.

Vật liệu cho bước này:

Bột nhômBột nhôm1 cái
Bari peroxitBari peroxit1 cái
Dải magieDải magie1 cái

Công cụ cần thiết:

Xô cát khôXô cát khô
4

Light it and stand back

Face shield on. Light the end of the ribbon and step well back. The fuse fires the charge and the reaction runs through it by its own heat.

Công cụ cần thiết:

Bật lửaBật lửa
Tấm che mặtTấm che mặt
Găng tay daGăng tay da
5

Break out the regulus

Let it cool completely. Break away the alumina slag on top and take out the button of chromium from the bottom. At most 103 g can form from 150 g of oxide.

Công cụ cần thiết:

BúaBúa
Găng tay daGăng tay da
Tấm che mặtTấm che mặt
Lọ thủy tinh có nắpLọ thủy tinh có nắp

Vật liệu

4
  • Tạm thời
  • Tạm thời
  • Tạm thời
  • Tạm thời

Công cụ yêu cầu

11

Bản thiết kế này làm ra

CC0 Phạm vi công cộng

Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.

Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.

Thảo luận

(0)

Đăng nhập để tham gia thảo luận

Đang tải bình luận...