Copper Concentrate: Sulphide Ore Stamped, Jigged and Tabled at the Anaconda Mill (Richards, Ore Dressing 1903)

Copper sulphide ore is too lean to smelt as mined. At the Anaconda mill it was screened, crushed under steam stamps, sorted by settling speed in rising water, and run over jigs and slime tables, where the heavy copper minerals sink and the light quartz and feldspar wash away. Result: concentrates of 12 to 20 % copper; 100 tons of ore gave 50 to 75 tons. The mill handled 2,500 to 2,700 tons a day. Source: Robert H. Richards, Ore Dressing vol. II (1903), pp. 984-986, Mill No. 42, Anaconda Copper Mining Company. Not given: the copper in the ore, water per ton. Picture drawn by Youblob.
Nâng cao
1 day

Hướng dẫn

1

Sort the ore

In the mine, pick the ore by hand into rich ore (straight to the smelter), hard concentrating ore and soft concentrating ore. The ore holds chalcocite, chalcopyrite, pyrite, enargite and blende in quartz and decomposed feldspar; the aim is to save the copper and silver without the zinc.

Vật liệu cho bước này:

Quặng đồng sunfuaQuặng đồng sunfua100 tons
2

Screen and pick

Pass each kind over vibrating grizzlies with 1 in spaces; hand-pick the oversize for rich ore. Screen the undersize in trommels: 6.35 mm round holes for hard ore; 12.7 mm then 6.35 mm for soft ore.

Công cụ cần thiết:

Sàng phân loạiSàng phân loại
Sàng thùng quaySàng thùng quay
3

Crush under steam stamps

Crush the coarse hard ore under steam stamps with screens of 4.76 x 9.52 mm slots, the soft ore under stamps with 12.7 mm round holes. Richards notes that steam stamps were later given up for these ores.

Công cụ cần thiết:

Máy nghiền chàyMáy nghiền chày
NướcNước
4

Classify and jig

Jig the coarse soft ore on 1-sieve Harz jigs. Send all fine ore to hydraulic classifiers with three spigots; each spigot feeds its own row of 2-sieve Collom jigs. The heavy concentrate is drawn from the jigs; middlings are crushed again.

Công cụ cần thiết:

Máy lắng quặng (jig)Máy lắng quặng (jig)
Máy phân cấp thủy lựcMáy phân cấp thủy lực
NướcNước
5

Table the slimes and collect

Run the classifier overflow over convex revolving slime tables. Gather all concentrates and settlings for the smelter: 12 to 20 % copper, 50 to 75 tons from 100 tons of ore. Tailings keep 1 1/4 to 2 % copper.

Công cụ cần thiết:

Bàn đãi bùn quayBàn đãi bùn quay
Bể lắngBể lắng

Vật liệu

1

Công cụ yêu cầu

8

Bản thiết kế này làm ra

CC0 Phạm vi công cộng

Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.

Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.

Thảo luận

(0)

Đăng nhập để tham gia thảo luận

Đang tải bình luận...