Electrolytic Capacitors: Borate Paper Wound with Formed Aluminium Foil and Vacuum-Impregnated (Danziger, US 2,107,780)
Ed

Tạo bởi

Ed

2. tháng Mười Một 2026FI
1
0
0
0
0

Electrolytic Capacitors: Borate Paper Wound with Formed Aluminium Foil and Vacuum-Impregnated (Danziger, US 2,107,780)

A dry electrolytic capacitor wound from aluminium foil and paper. The paper is first soaked in ammonium borate and dried, so the salt is already in its fibres. After winding, the bodies are soaked under heat and vacuum in borate dissolved in glycol, boxed and aged at 500 volts. Result: electrolytic capacitors. In the patent's tests these lost only 4.8 % of their capacity, against about 33 % for bodies made the ordinary way, and their power-factor loss rose 87 % on life test against 250 %. Source: H. I. Danziger and A. Di Giacomo, US 2,107,780 (1938). Unknown: how the anode foil is formed, which paper, the tab metal, and how the ammonium borate is made; the patent does not give them. Picture: Wikimedia Commons.
Nâng cao
1 day

Hướng dẫn

1

Salt the paper

Draw the paper strip through a saturated solution of ammonium borate in water, about 15 to 30 seconds for each part of it, then dry it at about 80 °C for about 15 seconds and reel it up. The salted paper keeps until needed. Unknown: which paper. Ours: a tray for the bath and a drying oven.

Vật liệu cho bước này:

Giấy cách tụ điệnGiấy cách tụ điện1 strip
Amoni boratAmoni borat1 to saturate

Công cụ cần thiết:

NướcNước
KhayKhay
Lò sấyLò sấy
2

Wind the bodies

On a winding machine, wind two aluminium foil strips with the salted paper between them onto a mandrel; at least one foil must already carry its electrolytic film. One paper strip is enough. Let the paper stand out at both ends, bring a connection tab out of each end, cut the strips and hold the body wound with a rubber band. Unknown: how the foil was formed, and the tab metal.

Vật liệu cho bước này:

Lá nhôm đã tạo màngLá nhôm đã tạo màng1 strip
Giấy nhômGiấy nhôm1 strip
Kim loại chưa rõKim loại chưa rõ2 tabs

Công cụ cần thiết:

Máy quấn tụ điệnMáy quấn tụ điện
Dây thunDây thun
3

Make the impregnant

Heat ethylene glycol to about 90 °C, then stir in powdered ammonium borate slowly and continuously until the solution reaches about 122 °C. Ours: a hot plate and thermometer.

Vật liệu cho bước này:

Etylen glycolEtylen glycol1 as required
Amoni boratAmoni borat1 as required

Công cụ cần thiết:

Bếp điện phẳngBếp điện phẳng
Nhiệt kếNhiệt kế
4

Soak under heat and vacuum

Rack the bodies in a vacuum tank heated to about 50 °C and draw about 745 mm of vacuum for about an hour to pull out air and moisture. Draw in the impregnant at about 85 °C, ease the vacuum to about 310 mm, and hold at about 85 °C for about another hour.

Công cụ cần thiết:

Thùng chân không có vỏ gia nhiệt bằng hơi nướcThùng chân không có vỏ gia nhiệt bằng hơi nước
Bơm chân khôngBơm chân không
Nhiệt kếNhiệt kế
5

Box and age

Take the bodies out, put them in cardboard containers, and age them at about 500 volts DC for about three hours.

Vật liệu cho bước này:

Ống bìa cứngỐng bìa cứng1 per capacitor

Công cụ cần thiết:

Nguồn một chiều cao áp (để bàn)Nguồn một chiều cao áp (để bàn)

Vật liệu

7

Công cụ yêu cầu

10

Bản thiết kế này làm ra

Blueprint liên quan

Các blueprint này chia sẻ kiến thức — kỹ thuật, vật liệu hoặc nguyên tắc

CC0 Phạm vi công cộng

Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.

Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.

Thảo luận

(0)

Đăng nhập để tham gia thảo luận

Đang tải bình luận...