Forged Hunting Axe (Hatchet)

A small one-handed axe forged from a 7/8 × 2-inch bar of good tool steel, best made by two people; a 6¾-inch bar gives two heads. The eye, about 9/16 × 1½ inches, is punched at a yellow heat with an eye punch and opened with drifts, the blade drawn out to a 3-inch edge and the head cut to length. The axe is annealed in lime or ashes, ground and buffed, then hardened from the hardening heat in tepid water and tempered by two hot iron bars laid on either side at the centre: dark purple for the blade, blue for the head.
Nâng cao
4–6 hours

Hướng dẫn

1

Mark and punch the eye

Mark the stock with chisel and centre punch. At a yellow heat, punch the eye with the narrow edge of the punch toward the blade; lift the punch after each blow to check it runs straight and to let it cool; a little fine coal in the hole stops it sticking. Punch nearly through, then finish from the other side.

Vật liệu cho bước này:

Thanh thép dụng cụ dẹtThanh thép dụng cụ dẹt1 cái

Công cụ cần thiết:

Đục dấu tâmĐục dấu tâm
Lò rèn của thợ rènLò rèn của thợ rèn
ĐeĐe
Đột nóngĐột nóng
Búa tạBúa tạ
Kìm rènKìm rèn
2

Drift and draw out

Drive in a tool-steel drift, hammer the bulges down to the bar's size and smooth with a flatter; take the drift out before each reheat. Use two drifts, the first 3/8 inch narrower. Draw out the blade, driving the drift back in as the eye stretches so no cold shut forms.

Công cụ cần thiết:

Đột nong lỗĐột nong lỗ
Búa làm phẳng của thợ rènBúa làm phẳng của thợ rèn
Búa rèn camBúa rèn cam
3

Shape and trim

Shape the blade with a heavy hammer and flatter and form its edge. Cut the head from the bar, draw it to size, cut it to length, then trim the blade to shape.

Công cụ cần thiết:

Búa rènBúa rèn
Búa làm phẳng của thợ rènBúa làm phẳng của thợ rèn
Đục nóngĐục nóng
4

Anneal and grind

Heat to a full red and anneal in lime or ashes. When cold, grind on an emery wheel and finish on a buffing wheel.

Công cụ cần thiết:

Lò rèn của thợ rènLò rèn của thợ rèn
Máy mài để bànMáy mài để bàn
5

Harden and temper

Heat very slowly to the hardening heat and cool in tepid water. Draw the temper with two hot iron bars laid on either side at the centre; when the blade is dark purple and the head blue, cool quickly in water.

Công cụ cần thiết:

Lò rèn của thợ rènLò rèn của thợ rèn
Thùng tôi nướcThùng tôi nước
Kìm rènKìm rèn
6

Handle

Shave the handle stock to fit the eye tightly, drive the head on, saw a kerf in the handle's top and drive a glued hardwood wedge into it. Trim flush and oil the handle.

Vật liệu cho bước này:

Phôi gỗ cứng làm cánPhôi gỗ cứng làm cán1 cái
Chêm gỗ cứngChêm gỗ cứng1 cái
Dầu lanhDầu lanh10 ml

Công cụ cần thiết:

Bào hai tay nắmBào hai tay nắm
Cưa xẻ hai ngườiCưa xẻ hai người
Ê tô bàn nguộiÊ tô bàn nguội

Vật liệu

4

Công cụ yêu cầu

16

Bản thiết kế này làm ra

Blueprint liên quan

Các blueprint này chia sẻ kiến thức — kỹ thuật, vật liệu hoặc nguyên tắc

CC0 Phạm vi công cộng

Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.

Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.

Thảo luận

(0)

Đăng nhập để tham gia thảo luận

Đang tải bình luận...