Lactide: Lactic Acid Condensed and Cracked under Vacuum, Recrystallised
Charlie

Tạo bởi

Charlie

19. tháng Mười 2026DE
12
0
0
0
0

Lactide: Lactic Acid Condensed and Cracked under Vacuum, Recrystallised

Lactide is the ring-shaped double molecule of lactic acid, the monomer from which PLA is made. Schneider's du Pont patent (US 2,703,316, 1955) drives the water out of lactic acid, condenses it under vacuum to a syrupy low polymer, then heats that to 200–250 °C at 8–10 mm so that lactide distils off. For a tough plastic it must be very pure: recrystallise it from ethyl acetate until it melts at 120 °C or higher (best 123–125 °C). The picture: our diagram.
Nâng cao
1–2 days

Hướng dẫn

1

Drive off the water

Distil the lactic acid at atmospheric pressure at 120–130 °C until nearly all the water of dilution has gone.

Vật liệu cho bước này:

Axit lactic (kỹ thuật)Axit lactic (kỹ thuật)1 cái

Công cụ cần thiết:

Bình cầu đáy trònBình cầu đáy tròn
Dàn ống ngưng tụDàn ống ngưng tụ
Bếp điện phẳngBếp điện phẳng
Bể dầuBể dầu
Nhiệt kế phòng thí nghiệmNhiệt kế phòng thí nghiệm
2

Condense under vacuum

Continue distilling under 17–35 mm of mercury. Water of esterification comes off and the acid becomes a syrupy low polymer (polylactic acid).

Công cụ cần thiết:

Bơm chân khôngBơm chân không
Đồng hồ chân khôngĐồng hồ chân không
Bẫy lạnhBẫy lạnh
Bể dầuBể dầu
Nhiệt kế phòng thí nghiệmNhiệt kế phòng thí nghiệm
3

Crack to lactide

Lower the pressure to 8–10 mm and raise the temperature to 200–250 °C. Lactide distils at 130–140 °C (10–13 mm) and sets to a soft crystalline solid.

Công cụ cần thiết:

Bơm chân khôngBơm chân không
Đồng hồ chân khôngĐồng hồ chân không
Dàn ống ngưng tụDàn ống ngưng tụ
Bể dầuBể dầu
Nhiệt kế phòng thí nghiệmNhiệt kế phòng thí nghiệm
Găng tay chịu nhiệtGăng tay chịu nhiệt
4

Recrystallise from ethyl acetate

Recrystallise the crude lactide from ethyl acetate, filter and dry. Repeat: in the patent the melting point rose from 114–115 °C after the first crystallisation to 118, 123–124 and 124–125 °C after the fourth.

Công cụ cần thiết:

Etyl axetatEtyl axetat
Cốc thủy tinh chịu nhiệtCốc thủy tinh chịu nhiệt
Bếp điện phẳngBếp điện phẳng
Phễu Büchner (bằng sứ)Phễu Büchner (bằng sứ)
Giấy lọcGiấy lọc
Kính chống hóa chất bắnKính chống hóa chất bắn
5

Check the melting point

Put a few crystals in a capillary tube and warm slowly. Lactide melting at 120 °C or above is fit for making PLA; below 120 °C it gives a brittle polymer.

Công cụ cần thiết:

Ống mao dẫn thủy tinhỐng mao dẫn thủy tinh
Nhiệt kế phòng thí nghiệmNhiệt kế phòng thí nghiệm
Bể dầuBể dầu

Vật liệu

1

Công cụ yêu cầu

15

Bản thiết kế này làm ra

CC0 Phạm vi công cộng

Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.

Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.

Thảo luận

(0)

Đăng nhập để tham gia thảo luận

Đang tải bình luận...