Saw File: Three-Square, Forged in a Boss, Cut by Hand and Hardened (Ure, 1839)
Forge

Tạo bởi

Forge

4. tháng Mười Một 2026NO
28
0
0
0
0

Saw File: Three-Square, Forged in a Boss, Cut by Hand and Hardened (Ure, 1839)

The file for sharpening saw teeth as Sheffield made it by hand: a three-square (triangular) bar of cast steel, not tapering, forged in a V-shaped boss, its teeth cut one by one with a chisel and hammer, then hardened under a coat of animal carbon and salt and quenched in cold spring water. Ure says saw files in particular should be hardened with the carbon mixture, so they will cut iron and steel. Not given: sizes and teeth per inch. Source: A. Ure, Dictionary of Arts, Manufactures, and Mines (1839), File. Picture: our drawing.
Nâng cao
Unknown

Hướng dẫn

1

Forge the blank

Draw cast steel out square at the forge, then lay it with one angle down in a boss whose recess has two sides meeting at an angle, so the hammer forms one side and the boss the other two. Keep it the same size along its length (saw files are not tapered).

Vật liệu cho bước này:

Thép nồi nấuThép nồi nấu1 cast steel bar
Kích thước chưa rõKích thước chưa rõ1 cái

Công cụ cần thiết:

Lò rèn của thợ rènLò rèn của thợ rèn
Kìm rènKìm rèn
Khuôn dập dưới (swage dưới)Khuôn dập dưới (swage dưới)
BúaBúa
Búa tạBúa tạ
2

Cut the teeth

On an anvil with a flat, even face, hold the file down with a leather strap over each end, the workman's feet in the straps like stirrups. Cut the teeth with a chisel a little broader than the file, sharpened to about 20 degrees, struck with a hammer of 1 to 6 lb. For single cut, run a fine file lightly over the teeth to take off the roughness; for double cut, cut a second set nearly at right angles to the first.

Công cụ cần thiết:

Đe thépĐe thép
Dây daDây da
Đục nguộiĐục nguội
BúaBúa
Giũa kim loạiGiũa kim loại
3

Cut the other sides

To cut the next side, lay the file in a piece of lead-tin alloy with an angular groove, so the teeth already cut are not spoiled on the anvil.

Công cụ cần thiết:

Thiếc hàn chìThiếc hàn chì
Đe thépĐe thép
Đục nguộiĐục nguội
BúaBúa
4

Coat for hardening

Distil shoemakers' and curriers' leather refuse in an iron still and powder the bright coal left. Grind about equal parts by bulk of this carbon and salt to the consistence of cream with water and cover the file with it.

Công cụ cần thiết:

Bình cất bằng sắtBình cất bằng sắt
MuốiMuối
NướcNước
5

Harden

Hold the file by the tang in a fire of very small cokes, drawing it out often, until it is an even cherry red from tang to point. Plunge it straight down, quickly, into clear spring water as cold as possible.

Công cụ cần thiết:

Lò rèn của thợ rènLò rèn của thợ rèn
Than cốc luyện kimThan cốc luyện kim
Kìm rènKìm rèn
NướcNước
6

Clean and oil

Brush the file with water and powdered cokes until clean and metallic, wash it in two or three waters to take off all the salt, dip it in lime-water, dry it quickly before the fire and oil it while warm with olive oil containing a little oil of turpentine.

Công cụ cần thiết:

Than cốc luyện kimThan cốc luyện kim
NướcNước
Nước vôiNước vôi
Dầu ô liuDầu ô liu
Dầu thôngDầu thông

Vật liệu

2

Công cụ yêu cầu

17

Bản thiết kế này làm ra

CC0 Phạm vi công cộng

Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.

Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.

Thảo luận

(0)

Đăng nhập để tham gia thảo luận

Đang tải bình luận...