Neodymium Magnets, Sample 15: 63Fe-17B-20Nd Sintered (Sagawa 1988)
Neodymium magnets are iron, boron and neodymium. Sagawa's team at Sumitomo melted the three together, ground the casting to a powder finer than 10 µm, lined the grains up in a magnetic field while pressing them, and sintered the compact in argon. This is their sample 15, 63 % iron, 17 % boron and 20 % neodymium by atoms: 10.5 MGOe.
Source: M. Sagawa et al. (Sumitomo Special Metals), US 4,770,723 (1988). Unknown: how the pure iron, the ferroboron and the neodymium metal are made, and how the finished magnets are magnetised; the patent does not say. The 1 kg weights are our arithmetic from the patent's atomic percentages. Picture: the patent's Fig. 8.
Chuyên gia
2 days
Hướng dẫn
1
1
Weigh sample 15: 63 Fe, 17 B, 20 Nd
Weigh sample 15: 63 Fe, 17 B, 20 Nd
Sample 15 is 63 % iron, 17 % boron and 20 % neodymium by atoms. Use 99.9 % electrolytic iron, ferroboron (19.38 % B, 5.32 % Al, 0.74 % Si, 0.03 % C, the rest iron) and neodymium of 99.7 % or better. Ours: a 1 kg melt, by arithmetic: 426.8 g iron, 144.0 g ferroboron, 438.0 g neodymium. Unknown: how these three are made.
Vật liệu cho bước này:
Sắt điện phân426.8 g
Ferô-bo144 g
Kim loại neođim438 gCông cụ cần thiết:
Cân hai đĩa2
2
Melt by high frequency in argon and cast
Melt by high frequency in argon and cast
Melt the charge in a high-frequency (induction) furnace under argon and pour it into a water-cooled copper mould.
Công cụ cần thiết:
Lò cảm ứng
Nồi nấu bằng đất chịu lửa
Argon
Bình khí chịu áp suất
Khuôn đồng làm nguội bằng nước
Găng tay chịu nhiệt3
3
Stamp to 35 mesh, ball-mill to 3-10 µm
Stamp to 35 mesh, ball-mill to 3-10 µm
Crush the casting in a stamp mill until it passes a 35-mesh sieve. Then grind it in a ball mill for 3 hours, to 3-10 µm.
Công cụ cần thiết:
Máy nghiền chày
Bộ sàng (mắt theo cấp)
Máy nghiền bi sắt
Kính bảo hộ4
4
Press in a 10 kOe field at 1.5 t/cm²
Press in a 10 kOe field at 1.5 t/cm²
Line the powder up in a magnetic field of 10 kOe and press it at 1.5 tonnes per cm². Unknown: the size and shape of the magnets.
Công cụ cần thiết:
Máy ép trong từ trường5
5
Sinter in argon at 1000-1200 °C
Sinter in argon at 1000-1200 °C
Sinter the compacts at 1000-1200 °C for about one hour in argon, then let them cool. Sample 15 measured 6.6 kG remanence, 12.8 kOe coercivity and 10.5 MGOe.
Công cụ cần thiết:
Lò ống
Argon
Bình khí chịu áp suất
Găng tay chịu nhiệt6
6
Magnetise the magnets
Magnetise the magnets
Unknown: how the sintered magnets are magnetised. Sagawa measures them on a B-H tracer but gives no magnetising field or apparatus.
Công cụ cần thiết:
Phương pháp từ hóa chưa rõVật liệu
3- 426.8 gTạm thời
- 144 gTạm thời
- 438 gTạm thời
Công cụ yêu cầu
14- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
- Tạm thời
Bản thiết kế này làm ra
Blueprint liên quan
Các blueprint này chia sẻ kiến thức — kỹ thuật, vật liệu hoặc nguyên tắc
CC0 Phạm vi công cộng
Bản thiết kế này được phát hành theo CC0. Bạn tự do sao chép, sửa đổi, phân phối và sử dụng cho bất kỳ mục đích nào mà không cần xin phép.
Hỗ trợ nhà sáng tạo bằng cách mua sản phẩm qua bản thiết kế, nơi họ nhận Hoa hồng nhà sáng tạo do nhà bán hàng đặt, hoặc tạo phiên bản mới và kết nối trong bản thiết kế riêng để chia sẻ doanh thu.